ASTM A790 vs A789 vs A928 Duplex Pipe and Tube Standards

A practical guide to ASTM A790, A789 and A928 duplex stainless steel pipe and tube standards covering scope, manufacturing routes, grades, PREN, testing and ordering.

ASTM A790 vs A789 vs A928: Which Standard Governs Your Order?

ASTM A790 covers seamless and straight-seam welded duplex stainless steel pipe; ASTM A789 covers seamless and welded duplex stainless steel tubing; ASTM A928 covers electric-fusion-welded duplex pipe made with filler metal. Select the product form and manufacturing route first, then specify the UNS grade, dimensions, inspection requirements and governing edition.

These standards can cover both duplex and super duplex grades. A standard number alone does not identify the alloy, establish suitability for seawater or sour service, or confirm compliance with a pressure design code. This guide explains the distinctions that engineers, buyers and inspectors need when preparing a material requisition.

Updated: 28 October 2026. This guide explains the distinctions that engineers, buyers and inspectors need when preparing a material requisition for duplex stainless steel pipes and tubes.

Request a Duplex Pipe or Tube Quotation

ASTM A790 vs A789 vs A928 at a glance

Selection pointASTM A790 / A790MASTM A789 / A789MASTM A928 / A928M
Product formPipeTubingPipe
Manufacturing routeSeamless or automatic straight-seam welding without filler metal in original manufactureSeamless or welded without added filler metalElectric fusion welding with filler metal, subject to class provisions
Dimension specificationCommonly NPS and schedule; other dimensions permitted subject to complianceOutside diameter and average wall thickness, unless minimum wall is orderedSpecify pipe dimensions and wall requirements in the order
General requirementsASTM A999 / A999MASTM A1016 / A1016MASTM A999 / A999M
Main ordering distinctionPipe route, grade and dimensionsTubing dimensions and wall basisGrade, welding class and examination requirements

Sources: A790/A790M-24, Sections 1, 4, 5 and 6; A789/A789M-24, Sections 1, 3, 4 and 5; ASTM A928 official scope information. [1–3]

What ASTM A790 covers

ASTM A790/A790M is a product specification for seamless and straight-seam welded ferritic/austenitic stainless steel pipe for general corrosive service, with particular emphasis on resistance to stress corrosion cracking. Duplex describes the ferritic/austenitic material family; it does not mean that every grade has the same corrosion resistance. [1]

For original welded manufacture, A790-2024 specifies an automatic welding process without added filler metal. However, Section 15 permits filler-metal repairs to the weld seam under defined conditions. These include size and wall-thickness eligibility, limits on repair extent, welding controls, heat treatment and WR identification. Therefore, the statement that A790 pipe can never contain filler metal is incorrect. If a project prohibits weld repair, state that restriction in the purchase order. [1]

NPS and schedule are common ordering conventions, rather than an absolute boundary of the specification. A790 Section 1.3 permits other dimensions when the remaining requirements are met. Always state the actual dimensional standard or specified OD and wall thickness, including the applicable tolerances. [1]

What ASTM A789 covers

ASTM A789/A789M covers ferritic/austenitic stainless steel tubing for general corrosion resistance, with particular emphasis on stress corrosion cracking resistance. It permits seamless or welded manufacture without added filler metal. Common applications include heat exchanger tubing and instrumentation tubing, subject to the equipment specification and design code. [2]

A789-2024 orders are based on outside diameter and average wall thickness unless minimum wall thickness is specified. Average wall and minimum wall are different acceptance bases. Describing a tube only as nominal wall leaves an avoidable ambiguity. Tube dimensions also do not make a product automatically suitable for every heat exchanger or instrumentation system. [2]

For heat exchanger tubes, A789 is the relevant specification to evaluate among these three standards. The exchanger shell, connected piping and other components may require different specifications. For product context, see 2205 S32205 seamless pipe and 2507 S32750 seamless pipe.

What ASTM A928 covers

ASTM A928/A928M addresses duplex stainless steel pipe produced by electric fusion welding with filler metal. It is often considered for fabricated welded pipe where the required dimensions and available manufacturing capacity favor this route. Large diameter is a common procurement context, rather than a complete definition of its scope. [3]

The A928 class is a procurement requirement, not an optional descriptive label. Class provisions address welding arrangement, filler-metal use and radiographic examination. Do not reduce the class selection to a simple quality ranking or assume that every class requires the same examination. Check the selected class against the contractual edition and project requirements. [3]

A928 is distinct from A790 original autogenous welded manufacture. A permitted repair to A790 pipe does not, by itself, convert that pipe into A928 pipe.

How to choose seamless or welded duplex products

Start with the design code, equipment specification and project piping class. If these allow more than one route, compare the required dimensions, examination coverage, qualified manufacturing capability, availability and total installed cost.

Seamless pipe or tube eliminates a longitudinal manufacturing weld seam, but this does not remove the need for appropriate heat treatment, inspection or corrosion assessment. Welded products can be suitable for demanding service when the permitted route and required quality controls are satisfied. A seam alone is not a sufficient basis for acceptance or rejection. For a grade-level comparison, see our guide to the duplex vs super duplex grades, PREN and key differences.

For example, a requisition for duplex heat exchanger tubing should identify the tubing standard, OD, wall basis and length. A requisition for filler-metal-welded duplex process pipe should identify the pipe standard and A928 class as well as the grade and dimensions. Avoid selecting a route solely from generalized claims about pressure rating, price or offshore preference.

Duplex grades and mechanical requirements

UNS S31803 and UNS S32205 are commonly associated with 2205 duplex stainless steel. S32205 has tighter minimum chromium, molybdenum and nitrogen requirements in A790-2024. It is a distinct UNS designation, not a synonym for dual certification. Dual certification requires documented compliance with both specified grade requirements and the applicable product specification. [1]

UNS S32750 and UNS S32760 are widely used super duplex designations. Specify the UNS grade rather than relying only on a trade name or the phrase 25Cr super duplex. Confirm grade coverage in each product standard and contractual edition; the grade list in one standard must not be assumed to apply to another.

The following values are specified minimums from ASTM A790/A790M-24 Table 3 for the listed pipe grades. They are material acceptance properties, not allowable design stresses. [1]

UNS gradeMinimum yield strength MPaMinimum tensile strength MPa
S31803450620
S32205450655
S32750550800
S32760550750

The SI values above are taken from the standard, not calculated conversions. Use the applicable unit system independently and check the full table, including elongation, hardness and footnotes, before acceptance. For a wider cross-grade comparison, see our overview of the mechanical properties of duplex and super duplex stainless steel pipe.

PREN and its limitations

A commonly used pitting resistance equivalent expression is PREN = %Cr + 3.3 × %Mo + 16 × %N, using mass percentages. The expression and acceptance threshold must be stated because tungsten-containing grades may use a different calculation. A790-2024 Table 2 includes grade-specific PREN footnotes, including a tungsten-adjusted expression for S32760. [1]

PREN is a composition-based screening measure. It does not establish a safe operating temperature, a seawater service life or immunity to crevice corrosion. Do not assign a single guaranteed PREN to an entire grade from typical chemistry, or classify every 25Cr grade as interchangeable super duplex.

Heat treatment and testing requirements

A790-2024 provides grade-specific heat treatment requirements and defined alternatives. Its Section 6.3.2 also permits a specified HT-O supply condition subject to the stated requirements. A789-2024 requires heat-treated tubing and provides a defined alternative route for seamless tubes after hot forming. Avoid stating that every compliant product must undergo the same final furnace cycle after welding or forming. [1,2]

For A790-2024, Section 14 requires each pipe to undergo a hydrostatic or nondestructive electric test; for A789-2024, Section 10 provides the corresponding requirement for each tube. Unless the purchase order specifies otherwise, these clauses leave the choice to the manufacturer. Neither clause means that both tests are automatically mandatory. [1,2]

Mechanical test selection and sampling depend on the product specification and manufacturing route. Separate these base requirements from project additions such as impact testing, specified ferrite measurements, positive material identification, corrosion testing and enhanced examination.

When additional testing is needed, identify the method, specimen location, frequency, test conditions and acceptance criteria. Merely listing ASTM A923 or ASTM G48 does not define a complete inspection requirement. The selected method must be appropriate for the material and the property being assessed.

NORSOK M630 and project material data sheets

NORSOK M-630 provides material data sheets and element data sheets for piping. It should not be described simply as a universal offshore material-selection approval. Identify the exact MDS, revision, product form and grade required by the project. [4]

An ASTM product designation alone does not demonstrate compliance with an MDS. Requirements for ferrite, impact properties, corrosion testing, manufacturing qualification and documentation must be checked against the selected project documents. Avoid publishing a broad grade-to-MDS mapping without verifying the actual data sheet.

In particular, do not treat a single ferrite range or a generic 25Cr label as applicable to every base metal, weld metal, product form and NORSOK material data sheet.

ASTM ASME and EN specifications

SA-790, SA-789 and SA-928 are related ASME material specifications. For ASME work, verify the specification adopted by the governing Code edition, permitted material and product form, and any additional requirements. Do not assume that ASTM and ASME documents are identical across editions or that an ASTM certificate alone establishes ASME compliance.

For process piping, check the material acceptance and design rules in the applicable ASME B31.3 edition. For pressure vessels, check the applicable BPVC construction rules and material requirements. Product-standard tensile properties are not substitutes for code allowable stresses.

EN 10216-5 and EN 10217-7 are relevant European specification families to evaluate for seamless and welded stainless steel pressure tubes, respectively. Similar compositions or familiar grade cross-references do not establish automatic equivalence. Compare chemistry, delivery condition, dimensions, testing, documentation and regulatory acceptance before substitution.

Service suitability and temperature limits

A790 and A789 warn that these steels can embrittle during prolonged exposure to elevated temperatures. Neither product-standard designation supplies a universal maximum service temperature. Establish the permitted temperature range from the grade, duration of exposure, construction code and project requirements. Avoid presenting about 300°C as a universal design limit. [1,2]

For chloride-bearing water and seawater, evaluate temperature, chemistry, oxygen or oxidant exposure, crevices, deposits and operating conditions. Super duplex may be a candidate, but the name or PREN alone cannot establish suitability. For low-temperature service, confirm required toughness and impact qualification.

For H2S-containing environments, assess the applicable ISO 15156 / NACE MR0175 requirements for the material condition and service environment. A general sour-service statement, or passing a corrosion test alone, is not sufficient evidence of compliance. For a detailed review, see our article on chloride SCC and sour service cracking.

Duplex pipe and tube purchase order checklist

  1. Specify the product standard, edition, unit system and any governing ASME or project requirements.
  2. State the UNS grade and any required dual certification; identify the exact NORSOK MDS and revision when applicable.
  3. Identify seamless or welded manufacture and the A928 class where relevant; state any weld-repair restrictions.
  4. Define dimensions, tolerances, wall basis, quantity, length and end preparation.
  5. State the delivery condition, applicable heat treatment and surface finish.
  6. Specify any required choice of hydrostatic or nondestructive electric testing and additional examination.
  7. Define supplementary tests with their methods, frequency, specimen locations and acceptance criteria.
  8. Agree certification, traceability, marking, inspection intervention points and packaging requirements.

If EN 10204 type 3.1 or 3.2 documentation is required, specify it explicitly and define the inspection arrangements. Do not describe either certificate type as an automatic requirement of all three ASTM specifications.

Frequently asked questions

What is the main difference between ASTM A790 and A789

ASTM A790 is a pipe specification; ASTM A789 is a tubing specification. Both cover seamless and welded duplex products. The distinction affects dimensional ordering, general requirements and inspection, so the specifications are not interchangeable solely because the UNS grade matches. [1,2]

Can ASTM A790 pipe contain filler metal

A790-2024 prohibits added filler metal in original welded manufacture, but Section 15 permits filler-metal weld-seam repairs under defined conditions. Check the repair provisions and project restrictions before accepting or rejecting repaired pipe. [1]

When should ASTM A928 be specified

Evaluate A928 when the required duplex pipe is made by electric fusion welding with filler metal. Specify the class and verify the contractual welding and examination provisions. [3]

Is S32205 automatically dual certified to S31803

No. S32205 is a UNS grade designation. Dual certification must be supported by evidence that the supplied product meets both specified grades and the relevant product requirements. [1]

Does ASTM compliance also establish NORSOK compliance

No. Check the exact project MDS, revision and additional requirements. A certificate referring only to an ASTM product standard does not establish compliance with all applicable NORSOK requirements.

Is there one maximum service temperature for duplex stainless steel

No. The permitted service range depends on the grade, exposure duration, design code and project requirements. A generic temperature recommendation should not be used as a design value.

Request a duplex pipe or tube quotation

Send the product standard and edition, UNS grade, manufacturing route, dimensions, quantity and inspection requirements with your enquiry. For projects requiring NORSOK or additional corrosion testing, include the applicable MDS and acceptance criteria so the proposed supply can be checked against a defined specification.

Send Your Pipe or Tube Specification

Technical references

  • [1] ASTM A790/A790M-24. Scope and dimensions: Sections 1.1–1.4, PDF page 1. Ordering, general requirements, manufacture and heat treatment: Sections 4–6, PDF pages 2–3. Chemistry and PREN: Table 2 and footnotes, PDF page 4. Mechanical properties: Table 3, PDF page 5. Per-pipe testing: Section 14, PDF pages 6–7. Weld repair and identification: Section 15, PDF pages 7–8. doi.org/10.1520/A0790_A0790M-24
  • [2] ASTM A789/A789M-24. Scope, ordering, general requirements and manufacture: Sections 1, 3, 4 and 5, PDF page 1. Heat treatment: Section 6 and Table 2, PDF pages 1–2 and 4. Per-tube testing: Section 10, PDF page 3. doi.org/10.1520/A0789_A0789M-24
  • [3] ASTM International, A928/A928M official scope and class information. This guide uses scope-level distinctions; the complete contractual edition controls detailed acceptance. store.astm.org/a0928_a0928m-14r25.html
  • [4] Standards Norway, NORSOK materials standards catalogue, including M-630. Consult the project-specified standard and exact data sheet for detailed requirements. standard.no — NORSOK M materials

This guide provides an overview rather than a complete procurement specification. The cited editions identify the basis of the technical discussion; the edition specified by the contract and the governing design requirements control acceptance.

Share your love

Leave a Reply

Your email address will not be published. Required fields are marked *

Related product pages

Each linked page lists the sizes, applicable standard and the inspection documents we can supply.

Last reviewed: · Wenzhou Xinzhe Tech Co., Ltd. · Ask for a quotation