How to Choose Between Alloy 625, Alloy 825 and 800H/800HT
Shortlist Alloy 625 (UNS N06625) when chloride pitting, crevice corrosion or chloride stress corrosion cracking (SCC) governs the design. Consider Alloy 825 (UNS N08825) for many sulfuric and phosphoric acid streams. Consider Alloy 800H (UNS N08810) or 800HT (UNS N08811) when creep or stress rupture governs the design at elevated metal temperatures.
A material selection guide for engineers, specifiers and nickel alloy pipe and tube buyers. This guide compares Inconel 625, Incoloy 825 and Incoloy 800H/800HT as they are typically shortlisted for seamless nickel alloy pipe and tube, explains what separates the three grades, and shows what to include in an RFQ so that supplier quotations can be compared line by line.
The final grade depends on fluid chemistry, metal temperature, pressure, fabrication route and the governing design code, not on the alloy name alone.
Updated: 7 November 2026. Alloy data and product specifications cited in this guide were checked against the manufacturer technical bulletins listed under Technical references.
Nickel Alloy Comparison at a Glance
This section holds two tables: a service-condition screening matrix, then a side-by-side factor table. Use them to build a shortlist, not to approve a material. They show what each grade is selected for and what a buyer should confirm before an order is placed.
Service Condition Comparison Matrix
| Alloy and UNS | Temperature reference | Media and exposure | PREN screening | Typical applications |
|---|---|---|---|---|
| Alloy 625 (N06625) | 982 °C / 1,800 °F — upper end of the manufacturer’s stated service range | Seawater and chloride-bearing process fluids where pitting and crevice corrosion are concerns | ≈46–56 (Cr–Mo estimate) | Marine and offshore tubing, chemical process piping |
| Alloy 825 (N08825) | ≈540 °C / 1,000 °F — above this, prolonged exposure can reduce ductility and impact strength | Selected sulfuric and phosphoric acid streams. Check concentration, temperature and contaminants. | ≈28–35 (Cr–Mo estimate) | Acid process piping, pickling equipment, heat exchangers |
| Alloy 800H (N08810) | 982 °C / 1,800 °F — ASME VIII Div. 1 service via Code Case 1983. Verify the code edition and the allowable stress for the product, design life and conditions. | Hot oxidizing and carburizing gases. Check both process and furnace atmospheres. | Not a selection metric for hot gas service | Furnace tubing, reformer outlet piping and hot process equipment |
| Alloy 800HT (N08811) | 982 °C / 1,800 °F — maximum allowable stress values for service to 1800 °F are defined through ASME II-D and Code Case 1983. Verify the applicable code edition and conditions. | Hot oxidizing and carburizing gases with sustained mechanical loading | Not a selection metric for hot gas service | High-temperature furnace and petrochemical tubing where creep life governs |
Temperature figures describe different manufacturer references. For pressure design, verify the applicable code, product form, heat treatment, allowable stress, metal temperature and design life. The PREN screening figures use Cr + 3.3 × Mo with the published composition limits and omit nitrogen. These calculated ranges are composition estimates. For alloy selection, use corrosion data for the actual fluid and evaluate creep and hot gas damage separately.
Sources: 625 bulletin · 825 bulletin · 800H and 800HT bulletin · PREN formula and limits.
Side-by-Side Selection Factors
| Selection factor | Alloy 625 | Alloy 825 | Alloy 800H / 800HT |
|---|---|---|---|
| UNS designation | N06625 | N08825 | N08810 / N08811 |
| Chemistry family | Ni-Cr-Mo with Nb | Ni-Fe-Cr with Mo, Cu, Ti | Ni-Fe-Cr with controlled C, Al, Ti |
| Primary selection driver | Chloride corrosion resistance and strength | Aqueous acid corrosion resistance | Creep and rupture strength |
| Typical service | Marine and chemical process tubing | Acid process pipe and tubing | Furnace and hot process tubing |
| Seamless tube specification | ASTM B444 | ASTM B423 | ASTM B407 |
| Main check before purchase | Localized corrosion and delivery condition | Acid concentration and contaminants | Metal temperature, stress and service life |
Read the specification, not the grade name. Specification references identify the common seamless product routes; they are not complete purchase requirements. Confirm the ordered edition, exact grade, product form and delivery condition. Manufacturer bulletins provide background data and do not replace the governing specification. [1–3]
What Each Nickel Alloy Is
Trade names are not specifications. INCONEL and INCOLOY are separate Special Metals trademark families: INCONEL grades are nickel-chromium alloys, while INCOLOY grades are nickel-iron-chromium alloys. Buyers frequently search for “Inconel 825” or “Inconel 625 vs 825”, but an inquiry should identify Alloy 625 or Alloy 825 by its UNS number to avoid ambiguity. [1, 2]
Inconel 625 (UNS N06625): Chloride and Localized Corrosion Resistance
Alloy 625 is a nickel-chromium-molybdenum alloy strengthened by the stiffening effect of molybdenum and niobium on its nickel-chromium matrix, so no precipitation-hardening treatment is required. This combination gives high strength together with strong resistance to localized corrosion and chloride stress corrosion cracking, which is why marine components and chemical processing equipment are established applications. [1]
Two points matter from the first inquiry:
- Corrosion resistance is not immunity. Describe crevices, deposits, stagnant sections and cleaning chemicals, not only the bulk fluid, so that the proposed alloy addresses the likely damage mechanism.
- The published service range is not a design rating. The manufacturer describes service from cryogenic temperature to 982 °C (1800 °F). That broad metallurgical range does not establish a pressure design temperature; the allowable design temperature must be derived for the specific product condition and applicable code. [1]
Incoloy 825 (UNS N08825): Aqueous Acid Service
Alloy 825 is a nickel-iron-chromium alloy with molybdenum, copper and titanium additions, and it is especially associated with sulfuric and phosphoric acid service. Titanium stabilization, combined with suitable processing, improves resistance to intergranular attack; it does not guarantee that such attack cannot occur. [2]
- Acid service is chemistry-specific. Record concentration, temperature, impurities, aeration and cleaning cycles. A grade that performs well in one process stream can behave differently in another stream carrying the same acid name.
- High temperature is a limitation, not a design target. Exposure above about 540 °C (1000 °F) can cause microstructural changes that reduce ductility and impact strength, and for that reason the manufacturer states that Alloy 825 is not normally used where creep-rupture properties govern. This is a metallurgical consideration rather than a universal code limit. [2]
Incoloy 800H and 800HT (UNS N08810 / N08811): Creep and Rupture Duty
Alloy 800H and 800HT are controlled variants of the Alloy 800 family. Tighter chemistry control and a high-temperature anneal give them better creep and rupture strength than standard Alloy 800. Both grades require an average grain size of ASTM No. 5 or coarser; note that a larger ASTM grain-size number means a finer grain. [3]
Manufacturer chemistry limits set carbon at 0.05–0.10 % for 800H and 0.06–0.10 % for 800HT. For 800HT, combined aluminum and titanium is specified at 0.85–1.20 %. All values are mass percentages. [3]
Inconel 625 vs Incoloy 825: Which Alloy Fits the Environment
Alloy 625 and Alloy 825 are often shortlisted together because both are nickel alloys for corrosive aqueous duty, yet they solve different problems.
| Selection question | Alloy 625 | Alloy 825 |
|---|---|---|
| Dominant threat | Chloride pitting, crevice corrosion, chloride SCC | General and localized attack in acids |
| Typical media | Seawater, brine, chlorinated and chemical process streams | Sulfuric and phosphoric acid, mixed acid streams |
| Strength level | High, Mo- and Nb-strengthened | Moderate |
| Creep duty | Not the usual design basis; verify code limits | Not normally selected where creep-rupture governs |
Neither grade is universally better. Alloy 625 usually earns its material premium when chloride-driven localized corrosion, or a higher strength requirement, is the controlling damage mechanism. Where the threat is acid attack at moderate temperature, Alloy 825 frequently meets the duty at lower cost. In both cases, qualify the grade against the actual process stream before comparing price.
Incoloy 800H vs 800HT: What Actually Differs
Both grades belong to the same family and are ordered to ASTM B407; in practice they differ mainly in chemistry limits, so the deciding factor is the allowable stress each grade is granted at the design metal temperature under the governing code.
| Feature | 800H (N08810) | 800HT (N08811) |
|---|---|---|
| Carbon, % | 0.05–0.10 | 0.06–0.10 |
| Aluminum + titanium, % | 0.30–1.20 [3] | 0.85–1.20 [3] |
| Average grain size | ASTM No. 5 or coarser | ASTM No. 5 or coarser |
| Heat treatment | High-temperature anneal | High-temperature anneal |
| Typical selection | General high-temperature tubing | Higher-stress or longer-life furnace components |
When comparing Incoloy 800H vs 800HT, check the code allowable stress at the design metal temperature, the heat treatment and the certificate for the heat being supplied. In ASME service, 800HT is granted higher maximum allowable design stresses than 800H. The suffix alone does not establish suitability for a particular furnace location or operating life. [3]
How to Select Nickel Alloy Pipe and Tube
Step 1: Start with the Expected Damage Mechanism
Separate wet corrosion from high-temperature degradation. If localized attack in a chloride-bearing fluid is the main concern, assess Alloy 625 and Alloy 825 against representative corrosion evidence. If sustained load at high metal temperature controls the design, evaluate creep, rupture, oxidation and carburization before selecting an 800H or 800HT product.
Temperature alone does not select the grade. A hot component may also see corrosive condensate during shutdown, and a cooler component may see concentrated chemicals trapped under deposits.
Step 2: Define the Complete Operating Envelope
Record normal and upset temperatures, pressure, fluid composition, pH, chloride level, acid concentration, oxygen exposure, flow conditions and expected service life. Use tube-metal temperature where it differs from process-fluid temperature.
For H2S-containing oil and gas service, assess the applicable ISO 15156 or NACE MR0175 requirements against the actual material condition and environment. Neither the alloy name nor a general corrosion statement establishes sour-service compliance.
Step 3: Qualify Each Candidate Grade
Qualification is where a shortlist becomes a specification. Match every candidate against representative corrosion data and the code allowable stress at the design metal temperature, then confirm that it can be produced by the intended fabrication route. Spell out the delivery condition, grain size and testing scope on which the qualification depends, and record them in the purchase documents.
Where corrosion testing is required, agree the method and acceptance criteria up front: ASTM G48 for pitting and crevice corrosion, ASTM G28 for intergranular attack, and NACE TM0177 where sour service applies.
Step 4: Compare Installed Cost After Qualification
Request comparable quotations using the same size, length, tolerances, testing and certification scope. Alloy 625 can carry a material premium, but relative prices depend on product availability, order volume and market conditions, so obtain current quotations rather than relying on a fixed cost ranking.
A higher-strength alloy may permit a thinner wall only when the applicable design calculation supports it. Check allowable stress, corrosion allowance, manufacturing tolerance, external pressure, joining and minimum practical wall thickness before claiming weight or cost savings.
What to Include in a Nickel Alloy Pipe and Tube RFQ
- Grade and specification: exact alloy and UNS number, plus the required product specification and edition.
- Product form and dimensions: seamless or welded construction, outside diameter or nominal pipe size, wall thickness or schedule, length and dimensional tolerances.
- Delivery condition: heat treatment, and any required grain-size verification or additional material-condition restrictions.
- Service conditions: design temperature, pressure, process medium and any service-specific qualification requirements.
- Inspection and documentation: required inspection, pressure or nondestructive testing, acceptance criteria, traceability and material certificates.
A quotation for ASTM B444 Alloy 625 seamless tube is not directly comparable with a quotation for a welded product or a different delivery condition. Resolve those differences before comparing unit prices.
Example inquiry wording
Please quote 120 m of cold-worked seamless Alloy 625 tube, UNS N06625, to ASTM B444 Grade 1, 25.4 mm OD × 2.11 mm average wall, annealed and pickled, with EN 10204 type 3.1 certification and ASTM G48 Method A corrosion testing. State the edition, delivery condition and any permitted substitutions in your offer.
This example is an initial RFQ, not a complete purchase specification or a material recommendation for a particular duty. Before order placement, agree the controlling units, dimensional tolerances, test requirements, surface condition and acceptance criteria in writing.
Frequently asked questions
What is the difference between Inconel 625 and Incoloy 825?
Alloy 625 is a Ni-Cr-Mo-Nb alloy selected mainly for its high strength and its resistance to chloride pitting, crevice corrosion and chloride SCC. Alloy 825 is a Ni-Fe-Cr alloy with Mo, Cu and Ti, selected mainly for aqueous acid service such as sulfuric and phosphoric acid. [1, 2]
What is the difference between Incoloy 800H and 800HT?
Both are ordered to ASTM B407 and share the same grain-size requirement. 800HT has a slightly higher minimum carbon (0.06 % vs 0.05 %) and a combined aluminum plus titanium requirement of 0.85–1.20 % (800H: 0.30–1.20 %). Check the allowable stress for each grade at the design metal temperature under the governing code. [3]
Is Inconel 825 the correct alloy name?
The established trade name is INCOLOY alloy 825, with UNS designation N08825. INCONEL and INCOLOY are separate Special Metals trademark families: INCONEL grades are nickel-chromium alloys, while INCOLOY grades are nickel-iron-chromium alloys. Buyers frequently search for “Inconel 825” or “Inconel 625 vs 825”, but an inquiry should identify Alloy 625 or Alloy 825 by its UNS number to avoid ambiguity. [1, 2]
Is Alloy 625 always better than Alloy 825?
No. The relevant question is whether each candidate meets the corrosion and mechanical requirements of the service. Qualify the candidates first, then compare availability, fabrication scope and lifecycle cost.
Can Alloy 800 replace 800H or 800HT?
Can Alloy 825 replace Alloy 625 in seawater service?
Treat it as a new material assessment. Evaluate temperature, crevices, deposits, water chemistry, flow and shutdown conditions. Salinity or operating pressure alone is not sufficient justification for the change.
Why is Alloy 825 not used for creep duty?
Exposure above about 540 °C (1000 °F) can reduce ductility and impact strength. Alloy 825 is therefore generally avoided when creep-rupture properties govern the design. Where sustained load at high metal temperature governs, an 800H or 800HT grade is normally the better starting point. [2, 3]
Which standards should be listed for seamless nickel alloy tubing?
Choose the Grade with a Clear Service Specification
Use this comparison to build a shortlist, then validate the material against the complete operating envelope. A clear specification links the grade to its product form, delivery condition, inspection scope and design basis, which is what allows suppliers to quote on the same basis.
Wenzhou Xinzhe supplies seamless nickel alloy tube alongside austenitic stainless, duplex and super duplex tubing. For a focused material inquiry, send the process medium and composition, design temperature and pressure, pipe or tube dimensions, construction route and required certification. These details let a supplier answer with a technical proposal rather than a bare price.
Request an Inconel 625, Incoloy 825 or 800H/800HT quotation
Send the UNS grade, product specification and edition, pipe or tube dimensions with the wall basis, delivery condition, testing scope and certification requirements with your enquiry. Quotations are prepared against that specification so that offers from different suppliers can be compared line by line.
Technical references
- [1] Special Metals. INCONEL alloy 625. Publication SMC-063, August 2013. Introduction, composition and specifications. specialmetals.com — INCONEL alloy 625 bulletin
- [2] Special Metals. INCOLOY alloy 825. Publication SMC-030, September 2004. Introduction, mechanical properties and specifications. specialmetals.com — INCOLOY alloy 825 bulletin
- [3] Special Metals. INCOLOY alloys 800H and 800HT. Alloy development, chemistry, grain size and specifications. specialmetals.com — INCOLOY alloys 800H and 800HT bulletin
This guide provides an overview rather than a complete procurement specification. The cited editions identify the basis of the technical discussion; the edition specified by the contract and the governing design requirements control acceptance.
Related product pages
Each linked page lists the sizes, applicable standard and the inspection documents we can supply.
-
Inconel 625 seamless tube (UNS N06625)
ASTM B444 · Alloy 625 -
Inconel 625 seamless pipe (UNS N06625)
ASTM B444 · Alloy 625 -
Incoloy 825 seamless tube (UNS N08825)
ASTM B423 · Alloy 825 -
Incoloy 825 seamless pipe (UNS N08825)
ASTM B423 · Alloy 825 -
Incoloy 800H seamless tube (UNS N08810)
ASTM B407 · Alloy 800H -
Incoloy 800H seamless pipe (UNS N08810)
ASTM B407 · Alloy 800H -
Incoloy 800HT seamless tube (UNS N08811)
ASTM B407 · Alloy 800HT -
Incoloy 800HT seamless pipe (UNS N08811)
ASTM B407 · Alloy 800HT
Last reviewed: · Wenzhou Xinzhe Tech Co., Ltd. · Contact the technical team