ASTM G48-25: Ferric Chloride Pitting and Crevice Corrosion Testing

ASTM G48-25 explained for buyers: the six ferric chloride test methods A to F, solution make-up, the 0.025 mm attack criterion, what a test report must state, and how to write the requirement into an RFQ.

ASTM G48 is the ferric chloride test method the stainless steel, duplex and nickel alloy trade uses to rank resistance to pitting and crevice corrosion initiation. It describes six procedures — Methods A, B, C, D, E and F — that expose a prepared specimen to a ferric chloride solution at a controlled temperature and then measure how much localised attack the surface has suffered. Nothing in it sets chemistry, mechanical properties or a pass/fail limit. It is a laboratory method, and it is read as one.

That distinction is where most confusion starts. A purchase order that says “ASTM G48” without naming a method letter and an acceptance temperature is not a test requirement — it is an invitation for the mill to choose the cheapest interpretation. Method A at 22 °C and Method E at 50 °C are both “G48”, and the numbers they produce are not interchangeable.

The current edition is ASTM G48-25: approved 1 October 2025, published October 2025, superseding G48-11(2020)ε1. The method was first issued in 1976 and sits under ASTM Committee G01 on Corrosion of Metals, Subcommittee G01.05 on Laboratory Corrosion Tests (DOI 10.1520/G0048-25). This guide works through what each method actually does, how the two test solutions differ, what the 0.025 mm attack threshold means, what a test report has to contain for two laboratories to be comparable, and the wording to put in an enquiry so that the certificate you receive answers the question you asked.

Updated: 17 November 2026. Clause references on this page were checked against the published English text of ASTM G48-25 on that date. This is an independent technical overview prepared for buyers and specifiers; it does not reproduce the standard. Acceptance decisions remain with the contract, the product specification and the governing design code.

The document at a glance

ItemDetail
DesignationASTM G48-25 — Standard Test Methods for Pitting and Crevice Corrosion Resistance of Stainless Steels and Related Alloys by Use of Ferric Chloride Solution
Edition historyCurrent edition approved 1 October 2025. Previous edition G48-11(2020)ε1. Originally approved 1976.
CommitteeASTM G01 on Corrosion of Metals, direct responsibility of Subcommittee G01.05 on Laboratory Corrosion Tests
MethodsSix: A and B (fixed-temperature pitting / crevice), C and D (critical temperature for nickel-base and chromium-bearing alloys), E and F (critical temperature for stainless steels)
OutputsMass loss, maximum pit depth, average of the ten deepest pits, pit density, crevice depth, number of attacked sites, critical pitting temperature (CPT), critical crevice temperature (CCT)
Acceptance limitNone. G48 defines how to test and what to report. The pass/fail temperature and criterion are set by the product specification, the project specification or the purchase order.

Which method you are actually asking for

The six methods fall into two families, and the difference matters more than the letters suggest. Methods A and B are fixed-temperature screening tests: the specimen sits at a stated temperature for a stated time, and the report gives mass loss, pit depth and pit density. Methods C, D, E and F are bracketing tests: the temperature is stepped up and down until the laboratory finds the lowest temperature at which attack of 0.025 mm or deeper appears, and that temperature is reported as a single number — CPT for pitting, CCT for crevice.

The second split is by alloy family. C and D were written for nickel-base and chromium-bearing alloys; E and F for stainless steels. That split is not bureaucratic. The nickel-base methods run a 72 h exposure per step because highly alloyed material needs the extra time to initiate; the stainless methods run 24 h per step. They also use different starting-temperature estimates. A CPT obtained by Method C and a CPT obtained by Method E can differ for the same heat, and comparing them without saying which was used is a common source of argument at inspection.

MethodMeasuresAlloy familyCrevice deviceSolutionDuration per step
APitting at a fixed temperatureStainless and nickel-baseNone — glass cradle6 % FeCl372 h
BPitting and crevice at a fixed temperatureStainless and nickel-baseTwo TFE-fluorocarbon blocks plus O-rings or rubber bands6 % FeCl372 h
CCPT — critical pitting temperatureNickel-base and chromium-bearingNone — glass cradle6 % FeCl3 + 1 % HCl72 h
DCCT — critical crevice temperatureNickel-base and chromium-bearingMultiple crevice assembly, 0.28 N·m6 % FeCl3 + 1 % HCl72 h
ECPT — critical pitting temperatureStainless steelsNone — glass cradle6 % FeCl3 + 1 % HCl24 h
FCCT — critical crevice temperatureStainless steelsMultiple crevice assembly, 1.58 N·m6 % FeCl3 + 1 % HCl24 h

Method A is a pitting test only. Method B is the reason the standard is worded “pitting and crevice”: the two blocks create four well-defined contact points and a reproducible crevice gap, so the same specimen surface yields both a general pit count and a crevice depth under the blocks. Method A is also the harsher test per unit of specimen area, because nothing shields the surface from the solution.

Why ferric chloride, and how far the result travels

Ferric chloride is not an arbitrary choice of aggressive salt. Section 4 explains that the solution is related to, but not the same as the liquid that develops inside an active pit or crevice on a ferrous alloy in a chloride environment — an acidic, concentrated chloride solution with a raised potential. Ferric ion supplies the oxidising power; the chloride concentration supplies the aggressiveness. Together they reproduce, in a beaker, the chemistry that keeps a pit growing.

That gives the test real predictive value in two situations: ambient-temperature natural seawater, and strongly oxidising low-pH chloride environments such as bleaching liquors and some chemical process streams. It is a poor predictor in others — reducing acids, chloride-free media, sour service, and any environment where the corrosion mechanism is stress corrosion cracking rather than pitting. The standard says this plainly in Section 4: no statement can be made about resistance in environments that do not contain chlorides.

Three further limits belong in the same paragraph, because they are the ones quoted out of context:

  • It accelerates initiation. All six methods were designed to start localised corrosion faster than most real environments, so the damage seen after 72 h in a beaker is generally worse than 72 h in service. A test result is a ranking, not a corrosion rate.
  • It says nothing about propagation. No method in G48 measures how fast an established pit grows, because the test stops when initiation is demonstrated.
  • Surface preparation changes the answer. Grinding and pickling can destroy the passive layer; a ground specimen and a pickled specimen of the same heat are not the same specimen. Note 1 in the standard accepts a 24 h air passivation after grinding or pickling as the practical way to minimise the difference — which is also why the finish has to be written into the enquiry, not left to the laboratory.

The two test solutions

Section 6 defines two solutions, and which one applies is decided by the method letter, not by the alloy.

SolutionMake-up (Clause 6)Used byNotes
6 % ferric chloride100 g reagent-grade FeCl3·6H2O dissolved in 900 mL Type IV reagent water (Specification D1193)Methods A and BAbout 6 % FeCl3 by mass. Filter through glass wool or filter paper to remove insolubles. No acid addition.
Acidified ferric chloride68.72 g FeCl3·6H2O in 600 mL reagent water plus 16 mL reagent-grade concentrated HCl (36.5–38.0 %)Methods C, D, E and FAbout 6 % FeCl3 and 1 % HCl by mass. The acid holds the pH in a controlled range across the test temperatures.

The acidified solution is the reason CPT values from C–F are not directly comparable with a fixed-temperature A result: it is a different, more tightly defined chemistry, chosen so that the only variable left in the bracketing is temperature.

Volume matters as well. The standard specifies 600 mL in a 1000 mL container for a standard specimen, 150 mL when a test tube is used instead, and a minimum of 5 mL per cm2 of specimen surface (about 30 mL per in2) for larger specimens. A laboratory that halves the solution volume to save reagent changes the test. For all bracketing methods the bath must hold temperature between 0 °C and 85 °C to within ±1 °C (Clause 5.2.2); the fixed-temperature methods are run at 22 ± 2 °C and 50 ± 2 °C, which are the two temperatures the standard recommends for evaluation.

Specimen preparation decides the number

Section 7 is short and almost entirely decisive. Two laboratories testing the same heat can differ by more than one 5 °C step if they read it differently.

  • Size. 25 mm by 50 mm (1 in. by 2 in.) is the recommended standard specimen, and every specimen in a series must share the same dimensions if comparisons are to mean anything. Keep the end-grain area small relative to the face area unless end-grain pitting is what you are testing — end grain pits far more readily than a wrought face.
  • Cut edges. If the specimen was sheared, the deformed metal must be removed by machining or grinding unless the corrosion resistance of the sheared edge is the subject of the test. As a rule, remove deformed material to the full thickness of the part.
  • Hole for Methods D and F. A hole has to be drilled and chamfered at the centre to take the bolt and insulating sleeve of the crevice assembly.
  • Finish. All faces polished to a uniform finish; 120 grit abrasive paper is the satisfactory standard. Wet polishing is preferred, and dry polishing must be slow enough to avoid overheating the surface. Sharp edges are rounded so they cannot cut the O-rings or rubber bands. Other finishes — mill finish, pickled, as-welded — may be tested deliberately, but then the report has to say so.
  • Measurement and cleaning. Measure the dimensions and calculate the exposed area; clean with magnesium oxide paste or equivalent, rinse, dip in acetone or methanol, air-dry; weigh to 0.001 g or better and keep in a desiccator until use.

For tube and pipe, the practical consequence is that a specimen cut from the wall carries a curved surface. The standard crevice formers are flat, so contact is not uniform on a small radius; contoured formers may be used, or the pitting method (A or C/E) chosen instead. That decision belongs in the test plan and in the report, not in a phone call after the results arrive.

Methods A and B: fixed-temperature screening

Method A is the test most often quoted on a mill certificate as “G48 Method A, 22 °C, 72 h, no pitting”. The sequence is: bring 600 mL of solution to temperature in a 1000 mL beaker, place the specimen in a glass cradle, immerse, cover with a watch glass, hold for 72 h, then rinse, scrub with a nylon brush under running water, dip in acetone or methanol, dry and weigh.

Method B adds the crevice. Two TFE-fluorocarbon blocks, 12.7 mm diameter and 12.7 mm high with 1.6 mm grooves, are fastened to the specimen with two O-rings (1.75 mm cross-section, about 20 mm and 30 mm inside diameter) or two rubber bands (No. 12 for the 25 mm direction, No. 14 for the 50 mm direction) of low-sulphur rubber. The specimen goes into a test tube holding 150 mL of solution, tilted at 45° so it slides to the bottom without trapping air. Gloves are worn so that no hand contact occurs on the test faces.

Two practical rules from Section 14 apply to both: a test must be discarded if an O-ring or rubber band breaks at any time during the exposure, and the crevice depth is measured at the points of contact under the blocks and under the rings — not just anywhere on the surface. Method B is also the method where specimen thickness affects the tightness of the crevice, so thickness is part of the result, not an afterthought.

Methods C to F: bracketing to a critical temperature

The bracketing methods answer a different question: not “did it pit at 22 °C” but “at what temperature does it start”. Both CPT and CCT are defined in Section 3 as the minimum temperature to produce attack at least 0.025 mm (0.001 in.) deep on the bold surface, with edge attack ignored. That single definition is what makes the reported number meaningful — and what makes it meaningless if the detection method is not stated.

The procedure starts from an estimate calculated from the alloy chemistry, rounded to the nearest 5 °C increment, and then walks the temperature until the threshold is crossed:

MethodStarting-temperature estimateRange and step
C — CPT, nickel-baseCPT = 2.5 × %Cr + 7.6 × %Mo + 31.9 × %N − 41.0Start at the nearest 5 °C, minimum 0 °C, maximum 85 °C
D — CCT, nickel-baseCCT = 1.5 × %Cr + 1.9 × %Mo + 4.9 × %Nb + 8.6 × %W − 36.2Same range; torque 0.28 N·m on the crevice assembly
E — CPT, stainlessSame equation as Method C, used as an estimate only24 h per step; no crevice device
F — CCT, stainlessCCT = 3.2 × %Cr + 7.6 × %Mo + 10.5 × %N − 81.024 h per step; torque 1.58 N·m on the crevice assembly

The estimate is a starting point, never a result. From there the rule is mechanical: if attack of 0.025 mm or deeper is found, drop the bath 5 °C; if it is not found, raise it 10 °C; each step uses a new specimen and fresh solution. The reported CPT or CCT is the lowest temperature at which attack appears. Because the step is asymmetric, the number is quantised to the step size — which is precisely why two laboratories can disagree by 5 °C without either being wrong.

Three further constraints belong in the same breath. Only one specimen may be in a container at a time. Method C and D run 72 h per step because highly corrosion-resistant nickel alloys can need that long to initiate; Methods E and F run 24 h. And Note 16 records the practical expectation that determining a critical temperature takes three to five replicate specimens per alloy and condition — a single specimen producing a single CPT is a screening result, not a qualification.

What counts as attack

Section 14 makes the difference between a result and an opinion. The examination is visual at low magnification — around 20× — supported by a probe: pits have to be probed with a needle, because localised attack is frequently occluded and a flat visual scan will miss it. Mass loss alone is not enough: the standard notes that a specimen losing very little mass can still be penetrated by a handful of small-diameter pits, while a mass loss of 0.0001 g/cm2 or more is an indicator that pitting or crevice attack is present and a visual examination is required.

What is recorded depends on the method. For Method A the maximum pit depth, the average of the ten deepest pits, the pit density per square centimetre on both 25 × 50 mm faces, and the mass loss in g/cm2. For Methods C and E, the maximum pit depth, which is then compared with the 0.025 mm threshold. For Methods B, D and F, the number of attacked sites on each side, the maximum depth, and the average depth under the blocks and at the ring contact points. Edge pits are disregarded unless end-grain attack is the subject.

That distinction — edge ignored, bold surface counted — is what makes the CPT definition usable. It also means a report that gives only “CPT 40 °C” without saying how pits were detected is not fully comparable to one that says “CPT 40 °C, needle-point micrometer, 20× pre-scan”. Note 25 in the standard makes the same point from the other direction: a shallow pit that a micrometer misses but a microscope sees makes the test more severe, not less.

What the test report has to state

Section 15 is the clause to quote when a certificate arrives without enough information to be checked. For every method the report must give the procedure used, the specimen size and surface preparation, the test time, the test temperature, the torque used to fasten the crevice assembly (Methods D and F), and the means by which pits or crevice attack were assessed.

Report itemRequired forWhy it matters
Method letter and edition (G48-25)All“G48” alone does not identify a test; A and E produce different numbers from the same heat
Specimen size, finish, edge conditionAllA pickled, ground or as-supplied surface is a different test
Temperature programme and step sizeC, D, E, F−5 / +10 °C bracketing quantises the result; without the steps the number cannot be reproduced
Torque on the crevice assemblyD (0.28 N·m), F (1.58 N·m)Torque sets crevice tightness, and crevice tightness sets CCT
Exposure time per stepAll72 h for C/D against 24 h for E/F is a defined difference, not a preference
Detection meansAllMicrometer, needle probe, 20× microscope — the same surface can give different severity
Pit depth, ten-deepest average, pit densityA (and C/E for maximum depth)Depth and frequency are more sensitive than mass loss
Attacked sites and depth at contactsB, D, FCrevice attack is only meaningful at the contact geometry
Mass loss in g/cm2A, BRapid comparison when attack is significant

Section 16 gives the expected scatter, and it is worth putting next to the acceptance number before arguing about a 5 °C shortfall. For the bracketing methods, the pooled reproducibility standard deviation and the 95 % confidence limit are: Method C 5 °C / 12 °C, Method D 6 °C / 16 °C, Method E 3 °C / 15 °C, Method F 3 °C / 9 °C. For Methods A and B the precision statement in the current edition records that the interlaboratory programme is still being determined.

What G48 does not tell you

  • Whether the material passes. There is no acceptance criterion in the standard. A mill certificate showing “G48 Method A, 22 °C, 72 h” and nothing else has told you the test was run, not that the result is acceptable to your specification.
  • How the pipe behaves in your plant. The test ranks initiation resistance in one specific chemistry. It is not a corrosion assessment for a process stream, and it does not replace one.
  • Anything about propagation, SCC or intergranular attack. Those are different mechanisms, tested by different standards. Sour service qualification is NACE MR0175 / ISO 15156 territory; intergranular susceptibility in austenitic grades is A262 territory.
  • Whether the heat treatment was correct. A CPT will drop if a duplex grade is badly annealed, so the test can flag a problem — but it does not identify the cause, and it is not a substitute for the microstructure and impact requirements in the product specification.
  • A number you can compare across sources. A datasheet CPT produced at 72 h per step by Method C and a certificate CPT produced at 24 h per step by Method E are not the same quantity. Compare method, edition, duration, torque and detection means, or do not compare at all.

How to write G48 into an enquiry

The requirement below is written for a duplex or super duplex line where the project wants a critical pitting temperature rather than a fixed-temperature screen. Change the method letter, temperature and specimen count to match the actual specification — the structure is the point.

“Corrosion testing: ASTM G48-25, Method E (critical pitting temperature), on specimens taken from the delivered pipe in the supplied condition. Specimen 25 mm × 50 mm, faces polished to 120 grit, edges rounded, tested in acidified ferric chloride solution (6 % FeCl3 + 1 % HCl) with 600 mL per 1000 mL container, one specimen per container, 24 h per step, bracketing in accordance with Section 12 (5 °C reduction on attack, 10 °C increase on no attack, fresh specimen and fresh solution at each step). Report per Section 15, including starting temperature, each step temperature, exposure time and the detection method used. Three specimens per heat. Acceptance: CPT not less than [40] °C, no specimen showing attack at 0.025 mm or deeper below that temperature. Testing at [laboratory]; witnessed by [third-party inspector].”

Four elements do most of the work, and each one is routinely missing:

  • The method letter and the edition. “ASTM G48” is not a requirement. “ASTM G48-25 Method E” is.
  • The acceptance temperature and the criterion. Either a fixed-temperature screen with an explicit “no pitting at 0.025 mm” statement, or a CPT minimum. State the number; do not let the mill choose it.
  • Specimen count and location. Three to five replicates per heat is the practical expectation for a CPT, and the specimen should come from the delivered product, not from a separate coupon.
  • Who tests and who witnesses. A laboratory result without an accredited report and, where the project requires it, third-party witnessing is difficult to defend at handover.

Five mistakes buyers make

  1. Ordering “G48” and accepting whatever method comes back. The cheapest interpretation is a 24 h Method A at 22 °C, which proves very little about a super duplex heat intended for 60 °C service.
  2. Comparing CPT values from different durations. Method C and D run 72 h per step; E and F run 24 h. A 72 h test will generally find attack at a lower temperature, so the two numbers are not interchangeable.
  3. Ignoring the crevice. Pitting resistance and crevice resistance are different properties, and in real gasketed or fouled service the crevice is the limiting case. If the application has crevices, specify Method B, D or F rather than A or C/E.
  4. Forgetting the surface condition. A ground specimen and a pickled specimen of the same heat can produce different CPTs. State the finish, and state whether the 24 h air passivation of Note 1 applies.
  5. Treating a laboratory ranking as a service guarantee. G48 says nothing about non-chloride media, propagation rate or cracking. Where the environment includes H2S, the governing document is NACE MR0175 / ISO 15156, not G48.

Frequently asked questions

What is the difference between G48 Method A and Method E?

Method A is a fixed-temperature pitting test: the specimen sits in 6 % ferric chloride at 22 ± 2 °C or 50 ± 2 °C for 72 h, and the report gives pit depth, pit density and mass loss. Method E is a bracketing test in acidified ferric chloride that steps the temperature until pitting of 0.025 mm appears, and reports a single critical pitting temperature. Method A answers “did it pit at this temperature”; Method E answers “at what temperature does it start”.

Is G48 a pass/fail test?

No. G48 defines the procedure and what to report; it contains no acceptance limit. The pass/fail temperature and criterion must come from the product specification, the project specification or the purchase order. A certificate that cites G48 without an acceptance criterion is evidence that a test was performed, not evidence that the material is acceptable.

Which method applies to duplex and super duplex stainless steel?

Methods E and F, because they were written for stainless steels; E gives CPT and F gives CCT. Method A at 22 °C is widely used as a fixed-temperature screen and appears in duplex qualification schemes, which is why “G48 Method A” shows up on duplex certificates. If the project asks for a critical pitting temperature, the method letter must be E, not A.

Why is 0.025 mm the threshold?

Because Section 3 defines CPT and CCT that way: the minimum temperature producing attack at least 0.025 mm (0.001 in.) deep on the bold surface, edge attack ignored. The value is a definition, not a tolerance. It exists so that a laboratory can decide objectively whether attack “started” at a given step, which is what makes a bracketing result reproducible at all.

How many specimens do I need for a reliable CPT?

Note 16 in the standard records the practical expectation of three to five replicate specimens per alloy and condition to determine a critical temperature. One specimen and one number is a screening result. For a project qualification, specify the count in the purchase order so the laboratory does not default to a single specimen.

Can G48 be used on welded specimens?

Yes, but the standard crevice formers are flat, so a weld cap or a curved tube surface does not give uniform contact. The standard notes that contoured formers may be used in that situation, or that the pitting method should be preferred. Whatever is chosen, the report must state the specimen form and the contact arrangement, otherwise the result cannot be compared with a flat-plate result on the same alloy.

Does G48 replace NACE MR0175 / ISO 15156?

No, and the two answer different questions. G48 ranks resistance to pitting and crevice initiation in ferric chloride. NACE MR0175 / ISO 15156 sets material limits and environmental restrictions for sour service, including hardness, chemistry and heat-treatment constraints, and it addresses sulphide stress cracking. Passing a G48 test says nothing about SSC qualification.

Why do two laboratories report different CPT values for the same heat?

Four reasons, all of them visible on the report if it follows Section 15: the temperature step size (5 °C reductions, 10 °C increases), the detection method (needle-point micrometer versus low-magnification microscope), the specimen finish and edge condition, and, for crevice tests, the torque on the assembly. Section 16 quantifies the scatter: reproducibility standard deviations of 5–6 °C for Methods C and D, 3 °C for E and F, with 95 % confidence limits of 12, 16, 15 and 9 °C respectively.

Can I quote a G48 result on a mill certificate instead of running a project test?

Only if the certificate states the method, edition, duration, temperature programme and detection means, and only if the specification allows historical or transferred results. Section 15 defines what has to be recorded; it does not create a right to substitute a previous test for a required one. Where the purchase order calls for testing on the delivered heat, a certificate for a different heat is not a substitute.

Related standards and technical guides

The product specifications that call up G48 testing, and the pages that explain what the grades behind the test actually are:

ASTM A312
ASTM A213
ASTM A269
ASTM A789
ASTM A790
ASTM B163
ASTM B444
ASTM B622
NACE MR0175 / ISO 15156
ISO 15156-3:2020
EN 10204 inspection certificates
Duplex 2205 (S31803 / S32205)
Super duplex 2507 (S32750)
Alloy 20 (N08020)
904L (N08904)
PREN calculator

Technical references

  • ASTM G48-25 — Standard Test Methods for Pitting and Crevice Corrosion Resistance of Stainless Steels and Related Alloys by Use of Ferric Chloride Solution. Approved 1 October 2025, published October 2025; supersedes G48-11(2020)ε1. Sections 1–17. DOI 10.1520/G0048-25. Publisher record
  • ASTM G46 — Guide for Examination and Evaluation of Pitting Corrosion (cited in Section 14 for the detailed examination of pit depth, density and crevice depth).
  • ASTM G193 — Terminology and Acronyms Relating to Corrosion (the definitions that apply where G48 is silent).
  • ASTM G1 — Practice for Preparing, Cleaning, and Evaluating Corrosion Test Specimens (cited for specimen cleaning and storage).
  • ASTM D1193 — Specification for Reagent Water (the Type IV water used to make both solutions).
  • ASTM E691 — Practice for Conducting an Interlaboratory Study to Determine the Precision of a Test Method (the basis of the precision statement in Section 16).
  • ASTM A262 — Practices for Detecting Susceptibility to Intergranular Attack in Austenitic Stainless Steels (the intergranular counterpart, frequently ordered alongside G48 on austenitic grades).
  • NACE MR0175 / ISO 15156 — the sour service documents that govern material selection where H2S is present; G48 does not substitute for them.

This page is an independent technical overview prepared for buyers and specifiers. It does not reproduce the text of ASTM G48 and is not a substitute for the published standard. The edition named in the contract, the product specification and the governing design code control acceptance.

Share your love

Leave a Reply

Your email address will not be published. Required fields are marked *

Last reviewed: · Wenzhou Xinzhe Tech Co., Ltd. · Ask for a quotation