ASTM A262-15(2021) sets out five laboratory practices for detecting susceptibility to intergranular attack in austenitic stainless steels. The supplied 20-page PDF contains Practices A, B, C, E and F: one electrolytic etch screening test and four hot-acid tests that either measure a corrosion rate or reveal intergranular cracking. This original guide explains what each practice measures, how the solutions and exposure periods are built, and how to state the requirement on a purchase order for pipe, tube and fittings.
ASTM A262-15(2021) PDF — Download Standard
What Is ASTM A262-15(2021)?
A262 is a set of test practices, not a material specification. It defines how a specimen is prepared, exposed and evaluated, and how the result is calculated and reported. It does not fix a universal pass number: the maximum permissible corrosion rate and the sensitizing treatment used before testing are left to agreement between producer and purchaser, which is why a purchase order that simply says “A262 tested” is incomplete.
Read the designation carefully. A262 is the fixed designation, -15 is the 2015 revision, and (2021) is a reapproval of that revision rather than a new technical edition. Quote the full string so a supplier cannot substitute an older print. The practices fall under ASTM Committee A01 on Steel, Stainless Steel and Related Alloys and are approved for use by agencies of the U.S. Department of Defense.
The five practices between them address three families of susceptibility: chromium carbide precipitation at grain boundaries, sigma or sigma-like phase, and end-grain attack. None of them predicts general corrosion, pitting or stress-corrosion cracking (Section 1.4), so an A262 report should never be presented as a general corrosion guarantee.
Standard at a Glance
| Item | A262-15(2021) |
|---|---|
| Designation | ASTM A262-15 (Reapproved 2021) |
| Title | Standard Practices for Detecting Susceptibility to Intergranular Attack in Austenitic Stainless Steels |
| Reapproval | 2021 reapproval of the 2015 revision; no new practice added |
| PDF contents | Practices A, B, C, E and F, 20 pages |
| Test types | One electrolytic etch classification test; four boiling-acid tests |
| Quantitative output | Practices B, C and F report a corrosion rate; Practice E is visual; Practice A is a structure classification |
| Units | SI is standard; inch-pound values in parentheses are approximate |
| Referenced documents | A370, A380/A380M, D1193, E3, ISO 3651-2, ASME BPVC Section IX |
| Scope limit | Austenitic stainless steels, wrought and cast; intergranular attack only |
The Five Practices at a Glance
| Practice | Medium and condition | Duration | Result | Targets |
|---|---|---|---|---|
| A — Oxalic acid etch | 10 % oxalic acid, electrolytic, 1 A/cm², room temperature | 1.5 min | Etch structure class (step, dual, ditch, and so on) | Screens for carbide-related susceptibility; acceptance only |
| B — Ferric sulfate-sulfuric acid | 50 % sulfuric acid plus 25 g ferric sulfate per 600 mL, boiling | 120 h | Corrosion rate, mm/month | Carbide precipitation in unstabilized grades; sigma in 321, 347 and cast Mo grades |
| C — Nitric acid (Huey) | 65 % nitric acid, boiling | 5 × 48 h (240 h) | Rate per period and average | Carbide, sigma-like phase and end-grain attack; nitric acid service |
| E — Copper-copper sulfate-16 % sulfuric | 1000 mL with 100 g copper sulfate and 100 mL sulfuric acid, boiling, copper shot | 15 h, then bend | Accept or non-accept by bend examination | Carbide precipitation in wrought grades and weld metal |
| F — Copper-copper sulfate-50 % sulfuric | 50 % sulfuric acid plus 72 g copper sulfate per 600 mL, boiling, metallic copper | 120 h | Corrosion rate, mm/month | Carbide precipitation in CF-3M, CF-8M and 316Ti |
The choice is not a matter of preference. Each practice has documented blind spots, listed in the nonmandatory Appendix X1, and selecting the wrong one can pass material that the correct test would reject.
Practice A: Oxalic Acid Etch Screening
Practice A is a metallographic screen. A polished cross-section is etched electrolytically in 10 % oxalic acid at 1 A/cm² for 1.5 minutes at room temperature, then examined at 250× to 500× and classified against the reference photomicrographs in the standard. The solution is 100 g of oxalic acid crystals in 900 mL of water; the specimen is polished through 600 grit (P1200) and should present a cross-sectional area of at least 1 cm² where the product allows.
The classification uses seven structure types, counting the two end-grain pitting levels separately. Step and dual structures are treated as acceptable for the grades listed in the relevant table; a ditch structure is suspect and must be followed by the hot-acid test. Castings and weld metal show isolated ferrite pools or interdendritic ditches instead of the wrought structures, and end-grain pitting I and II only matter when the nitric acid test is the destination.
| Etch structure | What the microstructure shows | How it is used |
|---|---|---|
| Step | Steps between grains, no ditches at boundaries | Acceptable for listed grades; no hot-acid test needed |
| Dual | Some ditches in addition to steps, no grain fully surrounded | Acceptable for listed grades as tabled |
| Ditch | One or more grains completely encircled by ditches | Suspect: the specified hot-acid test is mandatory |
| Isolated ferrite pools | Steps between austenite matrix and ferrite in castings and welds | Acceptable for CF grades where tabled |
| Interdendritic ditches | Deep interconnected ditches in castings and welds | Suspect for cast grades |
| End-grain pitting I and II | Deep pits on the exposed cross-section at 500× | Relevant only when screening for the nitric acid test |
Two limits matter commercially. First, Practice A is for acceptance only and explicitly must not be used to reject material (Section 4.1): a ditch structure means “run the hot-acid test”, not “scrap the heat”. Second, screening is valid only for the grades listed in the table that belongs to the hot-acid test being screened. Grades 316, 316L, 317, 317L, 321 and 347 cannot be screened before the nitric acid test, because sigma phase may be present without appearing in the etch structure.
For molybdenum-bearing grades where step structures are difficult to reveal, an ammonium persulfate electrolyte may be substituted (100 g in 900 mL of water, 5 to 10 minutes at 1 A/cm²).
Practice B: Ferric Sulfate-Sulfuric Acid, 120 h
Practice B is the general-purpose quantitative test for unstabilized austenitic grades. The 600 mL solution is built from 400 mL of reagent water, 236 mL of sulfuric acid (giving 49.4 % to 50.9 % total) and 25 g of ferric sulfate hydrate, boiled under reflux for 120 hours. Ferric sulfate is a specific additive that fixes the corrosion potential and may not be substituted; it is consumed at roughly 10 g per gram of stainless steel dissolved, so a fresh addition is required if the total mass loss in a flask exceeds 2 g.
The apparatus is part of the method. An Allihn condenser with at least four bulbs on a 1 L Erlenmeyer flask is specified, and cold-finger condensers are expressly prohibited because they return lower corrosion rates and can pass material that should be rejected. Specimens are 5 to 20 cm² total surface, ground to 120 grit (P120), freed of scale and heat tint, measured to 0.05 mm and weighed to 0.001 g.
Extra-low-carbon and stabilized grades are given a sensitizing treatment before testing, in the carbide-precipitation range of 650 °C to 675 °C; the most common treatment is 1 hour at 675 °C. Both the treatment and the maximum permissible rate are agreement items, not standard values. Rates are reported in millimetres per month using the mass-loss equation in Section 24, with density taken as 7.9 g/cm³ for chromium-nickel grades and 8.00 g/cm³ for chromium-nickel-molybdenum grades.
Practice B covers base metal only: welds, carburized or nitrided surfaces, mechanically deformed zones and heat-affected areas are outside its scope. It also does not detect sigma-related attack in wrought 316, 316L, 317 and 317L, nor end-grain attack, both of which are nitric acid phenomena.
Practice C: Nitric Acid (Huey), 240 h
Practice C is the test most often called the Huey test. The solution is 65.0 ± 0.2 mass % nitric acid, made by adding 108 mL of reagent water per litre of reagent nitric acid, and the standard sets impurity ceilings that matter: chloride 0.5 ppm maximum, fluoride 1 ppm, sulfate 1 ppm, iron 0.2 ppm. Fluoride contamination from a neighbouring nitric-hydrofluoric operation will inflate the corrosion rate, so the test must not share a hood with HF work.
The standard test is five boiling periods of 48 hours each with fresh acid every period, giving 240 hours of exposure; a combination of one 48-hour and two 96-hour periods may be substituted if the purchaser agrees. Solution volume must be at least 20 mL/cm² of specimen surface, typically about 600 mL, and each specimen normally gets its own flask. Rates are reported for every period in chronological order together with the average of the five, which is how a progressive rise in rate from sensitized grain boundaries becomes visible.
This is the only practice in the set that reveals sigma-related attack in molybdenum-bearing and stabilized grades and end-grain attack in all grades. That makes it the required test for nitric acid service, and the reason it should not be applied casually to extra-low-carbon molybdenum grades that will never see nitric acid.
Practice E: Copper-Copper Sulfate-16 % Sulfuric Acid, 15 h
Practice E is the fast qualitative option. The 1000 mL solution is 100 g of copper sulfate pentahydrate dissolved in 700 mL of water plus 100 mL of sulfuric acid, diluted to the mark, giving roughly 6 % copper sulfate and 16 % sulfuric acid. The specimen is embedded in electrolytic copper shot or grindings so that every surface is coupled, boiled for 15 hours, then bent and examined. Intergranular cracking or crazing in the bent area is evidence of susceptibility.
Because the result is a visual accept or non-accept rather than a rate, Practice E suits wrought products, weld metal and shop-floor decisions where a bend specimen can be sacrificed. ISO 3651-2 Method A may be used instead, with a minimum 15-hour period, unless the purchaser prohibits it; when a sensitizing treatment is required, T1 (700 ± 10 °C for 30 minutes, water quench) applies unless welded test pieces are agreed in the as-welded condition. The practice detects carbide-related attack and is blind to sigma phase and end-grain corrosion.
Practice F: Copper-Copper Sulfate-50 % Sulfuric Acid, 120 h
Practice F is the 120-hour variant for cast molybdenum-bearing grades and 316Ti. The 600 mL solution takes 400 mL of water, 236 mL of sulfuric acid and 72 g of copper sulfate pentahydrate, with a bright copper strip of about 3 × 20 × 40 mm immersed to hold the potential. Specimens are prepared as for Practice B and the mass loss is converted to a rate with the same equation. The practice detects chromium-carbide-related susceptibility in CF-3M, CF-8M and 316Ti and does not detect sigma phase, so it complements rather than replaces Practice C.
Which Practice Should the PO Call Out?
Appendix X1 is the selection guide, and it is the part of the standard most often skipped. In practice the choice follows from the grade and the service environment rather than from habit.
| Situation | Practice to specify | Why |
|---|---|---|
| Unstabilized wrought 304, 304L, 316, 316L, 317, 317L for general service | A screen, then B if suspect | Fastest route to a quantitative rate; A alone cannot reject |
| Any grade for nitric acid service | C | Only practice that reveals sigma and end-grain attack |
| 316L, 317L, 321, 347 before a nitric acid order | C, no A screening | Sigma may be invisible in the etch structure |
| Cast CF-3M, CF-8M, CG-3M, CG-8M | B, or F where carbides are the concern | Cast structures follow the cast-grade tables |
| Weld metal or a bend specimen is acceptable | E | 15 h plus bend; qualitative but fast |
| 321 or 347 in general service | B, or E for carbide-related attack | B detects the sigma-like phase in stabilized grades; Practice A is not tabulated as a screen for these grades |
| Duplex or super duplex | Not A262 | Scope is austenitic grades; use the duplex test standards |
Where a buyer needs both speed and defensibility, the common combination is Practice A as a screen followed by Practice B or Practice C on any suspect structure — which is exactly how the standard itself intends the practices to be used.
What a Test Report Must State
Because the acceptance values are agreement items, the report has to carry the agreement. A report that lists only “A262” and a pass verdict is difficult to defend in a claim. Check for the following.
- Full designation, including the reapproval year, and the practice letter used.
- Whether the specimen was sensitized, with temperature, time and cooling method, or tested as-received or as-welded.
- Specimen orientation, location relative to the weld or heat-affected zone, and surface preparation.
- Solution check: sulfuric acid concentration for B and F, nitric acid concentration for C, and the condenser type for B and F.
- Exposure schedule: total hours and number of periods, with individual and average rates for B, C and F.
- Calculation basis, including the density used for the rate equation.
- Specimen dimensions and balance resolution (0.001 g).
- Acceptance criterion, who set it, and the result for each specimen rather than a single heat-level statement.
- For Practice E: bend procedure and magnification of the examination, plus pass or fail.
On the purchasing side, the same list works in reverse: state the practice, the sensitizing condition, the maximum rate in a stated unit, and the reporting requirements in the RFQ so that two suppliers quote the same test. The manufacturing standard (for example ASTM A312 for pipe or ASTM A213 for tube) defines the product; A262 defines the test that supports the corrosion-resistance claim on the certificate.
Frequently Asked Questions
Is ASTM A262 the same as the Huey test?
No. The Huey test is Practice C within A262. The standard also contains the oxalic acid etch screen (A), the ferric sulfate-sulfuric acid test (B), and two copper-copper sulfate tests (E and F).
Why is there no Practice D?
The practice letters are historical. The 2015 revision as reapproved in 2021 contains Practices A, B, C, E and F only; there is no Practice D in the current text, so a quotation offering “A262 Practice D” is either an error or refers to a withdrawn method.
Can Practice A be used to reject a heat?
No. Practice A is for acceptance only. A ditch structure means the material must be tested in the specified hot acid, not that it fails the order.
Does A262 apply to duplex stainless steel?
No. The scope is austenitic stainless steels, wrought and cast. Duplex and super duplex grades are evaluated under their own test standards, including ASTM A923 for detrimental intermetallic phase and ISO 3651-2 for intergranular corrosion testing.
Which practice applies to 316L for a nitric acid plant?
Practice C. Grades 316, 316L, 317, 317L, 321 and 347 cannot be screened with Practice A before the nitric acid test because sigma phase may not be visible in the etch structure.
How long do the tests take?
Practice A is a 1.5-minute etch plus polishing and microscopy. Practice E is 15 hours plus bending. Practices B and F run 120 hours. Practice C runs 240 hours as five 48-hour periods, and a modified 48 + 96 + 96 hour schedule is possible by agreement.
Does passing A262 mean the pipe will not corrode in service?
No. The practices detect intergranular susceptibility only. General corrosion, pitting and stress-corrosion cracking require separate evaluation, and the operating environment still governs performance.
What does the 2021 date change?
It is a reapproval of the 2015 revision rather than a technical revision. Quote the full designation A262-15(2021) so that the edition supplied is unambiguous.
Related Standards and Engineering Resources
- ASTM A312 seamless and welded austenitic stainless steel pipe
- ASTM A213 seamless stainless steel boiler and heat exchanger tube
- ASTM A269 seamless and welded stainless steel tubing
- ASTM A790 duplex stainless steel pipe
- ASTM G48 ferric chloride pitting and crevice corrosion testing
- TP316L seamless stainless steel tube (UNS S31603)
- TP321H seamless stainless steel tube (UNS S32109)
- EN 10204 inspection certificates: 2.1, 2.2, 3.1 and 3.2
- Browse all standards