DIN 17751:2002-09 is the German standard that fixes the room-temperature mechanical properties of tubes made from wrought nickel and nickel alloys. Its German title is “Rohre aus Nickel und Nickel-Knetlegierungen — Eigenschaften”; the English title printed on the cover is “Tubes of wrought nickel and nickel alloys — Properties”. The September 2002 edition carries ICS 77.150.40 and replaces DIN 17751:1983-02.
The standard is deliberately narrow. It does not repeat chemical composition; it points to the DIN 17740 to DIN 17744 composition standards. It does not repeat dimensional tolerances; it points to DIN 59755. What it does provide is a single mechanical-property table — Tabelle 1 — that ties each Werkstoff number (2.xxxx) and condition code to a minimum tensile strength, 0.2 % and 1 % proof stress, elongation and Brinell hardness, banded by wall thickness.
This guide reproduces the property table for the grades most often ordered as seamless tube, explains the condition codes and hardness rules, and sets out what has to be stated on the purchase order so that a mill in Germany, Italy or China can quote the same material.
DIN 17751:2002-09 at a Glance
| Standard | DIN 17751:2002-09 (September 2002), ICS 77.150.40 |
| Title | Rohre aus Nickel und Nickel-Knetlegierungen — Eigenschaften / Tubes of wrought nickel and nickel alloys — Properties |
| Replaces | DIN 17751:1983-02 |
| Scope | Room-temperature mechanical properties of nickel and nickel alloy tubes within the wall-thickness bands of Tabelle 1 |
| Chemistry | Not in this standard: DIN 17740 (nickel), DIN 17742 (Ni-Cr), DIN 17743 (Ni-Cu), DIN 17744 (Ni-Mo-Cr) |
| Dimensions and tolerances | DIN 59755, cold-finished nickel and nickel alloy tubes |
| Test methods | DIN 50125 (tensile specimens), DIN EN 10002-1 (tensile test), DIN EN ISO 6506-1 (Brinell), DIN EN ISO 6507-1 (Vickers) |
| Property table | Tabelle 1, pages 4–5, 41 condition rows across four alloy families |
What Changed in the 2002 Edition
The foreword lists three substantive changes against the 1983 edition. Two grades were withdrawn — NiCr22Mo6Cu (2.4618) and NiCr21Mo6Cu (2.4641). Eleven materials were added. And the property data for the remaining grades was completely reworked, which means a certificate written to the 1983 edition cannot be read across to the 2002 table without checking each value.
That last point matters in procurement. A drawing that simply says “DIN 17751” is ambiguous if the order was first raised decades ago; the purchase order should quote DIN 17751:2002-09 in full.
Scope: What the Standard Does and Does Not Cover
Clause 1 states that the standard fixes the mechanical properties of tubes of nickel and nickel alloys for the dimensional ranges given in Tabelle 1. If tube outside those ranges is required with the properties of this standard, the properties have to be agreed at the time of ordering — they are not automatically extended.
Clause 3 adds that the purchaser selects the material and the delivery condition, and that the intended application and subsequent processing should be stated with the order. Clause 5 then hands chemistry to DIN 17740, DIN 17742, DIN 17743 and DIN 17744, clause 6 hands dimensions, limit deviations and form tolerances to DIN 59755, and clause 7 sets the mechanical test methods.
| Subject | Where it is specified | What that means for a buyer |
|---|---|---|
| Chemical composition | DIN 17740 (pure nickel), DIN 17742 (Ni-Cr), DIN 17743 (Ni-Cu), DIN 17744 (Ni-Mo-Cr) | The MTC has to cite the composition standard as well as DIN 17751, or the chemistry cannot be verified |
| Dimensions, limit deviations, form tolerances | DIN 59755 | Tolerances are not in DIN 17751; a “DIN 17751” order without DIN 59755 leaves size tolerance open |
| Tensile testing | DIN 50125 specimens, DIN EN 10002-1 method | Room-temperature tensile test, longitudinal direction |
| Hardness | DIN EN ISO 6506-1 (Brinell), DIN EN ISO 6507-1 (Vickers) | Brinell HBW 2.5/62.5 is the default; Vickers is the fallback with a 15 % allowance |
Material Numbers and Common Equivalents
DIN 17751 works with Werkstoff numbers (2.xxxx) and German short names, not UNS numbers. The table below lists the grades most often supplied as seamless tube. The UNS column is indicative only: it shows the alloy family a buyer is likely to recognise, but the formal equivalence has to be confirmed against the applicable ASTM or EN product specification and the mill certificate.
| Werkstoff no. | Short name | Family | Common UNS (indicative) |
|---|---|---|---|
| 2.4060 | Ni99.6 | Pure nickel | N02200 |
| 2.4061 | LC-Ni99.6 | Pure nickel, low carbon | N02201 |
| 2.4066 | Ni99.2 | Pure nickel | N02200 |
| 2.4068 | LC-Ni99 | Pure nickel, low carbon | N02201 |
| 2.4360 | NiCu30Fe | Nickel-copper | N04400 |
| 2.4361 | LC-NiCu30Fe | Nickel-copper, low carbon | N04400 |
| 2.4816 | NiCr15Fe | Nickel-chromium-iron | N06600 |
| 2.4817 | LC-NiCr15Fe | Nickel-chromium-iron, low carbon | N06600 |
| 2.4851 | NiCr23Fe | Nickel-chromium-iron | N06601 |
| 2.4633 | NiCr25FeAlY | Nickel-chromium, oxide-dispersion resistant | N06025 |
| 2.4951 | NiCr20Ti | Nickel-chromium, precipitation hardened | N06075 |
| 2.4600 | NiMo29Cr | Nickel-molybdenum | N10675 |
| 2.4617 | NiMo28 | Nickel-molybdenum | N10665 |
| 2.4602 | NiCr21Mo14W | Nickel-chromium-molybdenum-tungsten | N06022 |
| 2.4605 | NiCr23Mo16Al | Nickel-chromium-molybdenum | N06059 |
| 2.4606 | NiCr21Mo16W | Nickel-chromium-molybdenum-tungsten | N06686 |
| 2.4610 | NiMo16Cr16Ti | Nickel-molybdenum-chromium | N06455 |
| 2.4660 | NiCr20CuMo | Nickel-chromium-iron-copper | N08020 |
| 2.4675 | NiCr23Mo16Cu | Nickel-chromium-molybdenum-copper | N06200 |
| 2.4733 | NiCr22W14Mo | Nickel-chromium-tungsten-molybdenum | N06230 |
| 2.4819 | NiMo16Cr15W | Nickel-molybdenum-chromium-tungsten | N10276 |
| 2.4856 | NiCr22Mo9Nb | Nickel-chromium-molybdenum-niobium | N06625 |
| 2.4858 | NiCr21Mo | Nickel-chromium-iron-molybdenum | N08825 |
Tabelle 1 also covers NiCr29Fe (2.4642), NiCr28FeSiCe (2.4889), NiCr22Mo7Cu (2.4619) and NiMo23Cr8Fe (2.4710); the PDF should be consulted before ordering those grades.
Mechanical Properties: Tabelle 1
The property table is banded by wall thickness, not by outside diameter. Each row combines a material number, a condition code (Zustand, such as F37 or F69) and a heat-treatment name — weichgeglüht (soft annealed), halbhart (half-hard), hart (hard) or lösungsgeglüht (solution annealed). Values are minimums for Rm, Rp0.2, Rp1.0 and A5, and a maximum for Brinell hardness.
| Werkstoff | Zustand | Heat treatment | Wall (mm) | Rm min (N/mm²) | Rp0.2 min (N/mm²) | Rp1.0 min (N/mm²) | A5 min (%) | HBW max |
|---|---|---|---|---|---|---|---|---|
| 2.4060 Ni99.6 | F37 | Soft annealed | 0.5–5 | 370 | 100 | 125 | 40 | 130 |
| 2.4060 Ni99.6 | F49 | Half-hard | 0.5–4 | 490 | 290 | — | 20 | — |
| 2.4060 Ni99.6 | F59 | Hard | 0.5–4 | 590 | 490 | — | 2 | — |
| 2.4061 LC-Ni99.6 | F34 | Soft annealed | 0.5–5 | 340 | 80 | 105 | 40 | 130 |
| 2.4061 LC-Ni99.6 | F43 | Half-hard | 0.5–4 | 430 | 150 | — | 20 | — |
| 2.4061 LC-Ni99.6 | F54 | Hard | 0.5–4 | 540 | 430 | — | 5 | — |
| 2.4066 Ni99.2 | F37 | Soft annealed | 0.5–5 | 370 | 100 | 125 | 40 | 130 |
| 2.4068 LC-Ni99 | F34 | Soft annealed | 0.5–5 | 340 | 80 | 105 | 40 | 130 |
| 2.4360 NiCu30Fe | F45 | Soft annealed | 0.5–5 | 450 | 180 | 210 | 35 | 140 |
| 2.4360 NiCu30Fe | F55 | Half-hard | 0.5–4 | 550 | 300 | — | 25 | — |
| 2.4360 NiCu30Fe | F70 | Hard | 0.5–4 | 700 | 650 | — | 2 | — |
| 2.4361 LC-NiCu30Fe | F43 | Soft annealed | 0.5–5 | 430 | 160 | 185 | 35 | 120 |
| 2.4816 NiCr15Fe | F50 | Solution annealed | 0.5–5 | 500 | 180 | 210 | 35 | 185 |
| 2.4816 NiCr15Fe | F55 | Soft annealed | 0.5–5 | 550 | 200 | 230 | 30 | 195 |
| 2.4817 LC-NiCr15Fe | F50 | Solution annealed | 0.5–5 | 500 | 170 | 200 | 35 | 185 |
| 2.4851 NiCr23Fe | F55 | Solution annealed | 0.5–5 | 550 | 205 | 235 | 30 | 220 |
| 2.4851 NiCr23Fe | F60 | Soft annealed | 0.5–5 | 600 | 240 | 270 | 30 | 220 |
| 2.4633 NiCr25FeAlY | F65 | Solution annealed | 0.5–3 | 650 | 270 | 330 | 30 | — |
| 2.4951 NiCr20Ti | F65 | Solution annealed | 0.5–5 | 650 | 240 | 270 | 25 | 230 |
| 2.4600 NiMo29Cr | F75 | Solution annealed | 0.5–5 | 750 | 340 | 380 | 40 | 250 |
| 2.4602 NiCr21Mo14W | F69 | Solution annealed | 0.5–5 | 690 | 310 | 335 | 40 | 240 |
| 2.4605 NiCr23Mo16Al | F69 | Solution annealed | 0.5–3 | 690 | 340 | 380 | 40 | 240 |
| 2.4606 NiCr21Mo16W | F69 | Solution annealed | 0.5–3 | 690 | 310 | 335 | 40 | 240 |
| 2.4610 NiMo16Cr16Ti | F69 | Solution annealed | 0.5–5 | 690 | 275 | 295 | 40 | 240 |
| 2.4617 NiMo28 | F76 | Solution annealed | 0.5–5 | 755 | 340 | 360 | 40 | 250 |
| 2.4619 NiCr22Mo7Cu | F62 | Solution annealed | 0.5–5 | 620 | 240 | 260 | 35 | 240 |
| 2.4660 NiCr20CuMo | F55 | Soft annealed | 0.5–5 | 550 | 240 | 270 | 40 | 220 |
| 2.4675 NiCr23Mo16Cu | F69 | Solution annealed | 0.5–5 | 690 | 280 | 300 | 45 | 240 |
| 2.4710 NiMo23Cr8Fe | F72 | Solution annealed | 0.5–3 | 720 | 320 | 360 | 40 | 240 |
| 2.4733 NiCr22W14Mo | F76 | Solution annealed * | 0.5–5 | 760 | 310 | — | 35 | — |
| 2.4819 NiMo16Cr15W | F69 | Solution annealed | 0.5–5 | 690 | 280 | 300 | 40 | 240 |
| 2.4856 NiCr22Mo9Nb | F69 | Solution annealed | 0.5–5 | 690 | 275 | 315 | 35 | 200 |
| 2.4856 NiCr22Mo9Nb | F83 | Soft annealed | 0.5–5 | 830 | 415 | 445 | 30 | 240 |
| 2.4858 NiCr21Mo | F55 | Soft annealed | 0.5–8 | 550 | 235 | 265 | 30 | 190 |
* For 2.4733 in condition F76 the solution annealing temperature is restricted to 1 204 °C to 1 246 °C (footnote b of Tabelle 1). A dash means the standard sets no requirement for that column.
Hardness: The 15 % Vickers Allowance
Clause 7 sets the hardness method. Brinell hardness is measured with a 2.5 mm ball and a test force of 612.9 N — written HBW 2.5/62.5 — in accordance with DIN EN ISO 6506-1. If Brinell measurement is not possible, Vickers hardness may be measured to DIN EN ISO 6507-1, and in that case the Vickers value is permitted to be 15 % higher than the Brinell limit in the table.
Two practical consequences follow. First, a Vickers reading that sits between the Brinell limit and 1.15 times that limit is still compliant, so a certificate cannot be rejected on a direct number-to-number comparison. Second, every measured value must be rounded to the same precision as the limit before comparison, applying the rounding rule of DIN 1333.
What to Put on the Purchase Order
Clause 3 leaves material and delivery condition to the purchaser and recommends stating the intended use and subsequent processing. A complete order line for DIN 17751 tube normally carries:
- The standard, written in full: DIN 17751:2002-09.
- The material number and short name, for example 2.4856 NiCr22Mo9Nb, together with the composition standard — DIN 17744 for the Ni-Cr-Mo family.
- The delivery condition and its code: F69 solution annealed, F55 soft annealed, F83 for the higher-strength 625 condition, and so on.
- Dimensions: outside diameter and wall thickness, ordered to DIN 59755 tolerances, plus length and end finish.
- The tests required, and whether a third-party inspection or a specific inspection document is needed.
- The intended service, particularly where chlorides, reducing acids or high temperature are involved, so that the mill can flag a grade mismatch before rolling.
Frequently Asked Questions
Does DIN 17751 contain chemical composition limits?
No. Clause 5 refers composition to DIN 17740 for pure nickel, DIN 17742 for nickel-chromium alloys, DIN 17743 for nickel-copper alloys and DIN 17744 for nickel-molybdenum-chromium alloys. A mill certificate that cites only DIN 17751 therefore does not demonstrate chemistry compliance; the composition standard has to appear on the certificate as well.
Which is the correct delivery condition for 2.4856 (NiCr22Mo9Nb)?
Tabelle 1 lists two rows for 2.4856. Condition F69 (solution annealed) requires Rm of at least 690 N/mm², Rp0.2 of at least 275 N/mm², elongation of 35 % and Brinell hardness not above 200. Condition F83 (soft annealed) raises the strength floors to 830 N/mm² and 415 N/mm² with 30 % elongation and a 240 HBW ceiling. State the condition code on the order; the two are not interchangeable.
Can a Vickers hardness result be rejected because it exceeds the HBW limit?
Not directly. Clause 7 allows Vickers testing where Brinell is not possible and permits the Vickers value to be up to 15 % above the Brinell limit. Compare the rounded Vickers result with 1.15 times the table value before drawing a conclusion.
Does DIN 17751 specify dimensional tolerances?
No. Clause 6 refers dimensions, limit deviations and form tolerances to DIN 59755. If an enquiry asks only for “DIN 17751 tube”, the size tolerance is undefined until DIN 59755 or a drawing tolerance is added.
Is a DIN 17751 grade the same as the equivalent ASTM grade?
They are related but not identical documents. DIN 17751 sets mechanical properties only and refers chemistry and tolerances to other German standards, while ASTM product specifications such as B161, B163, B165, B167, B444, B622 and B829 set chemistry, properties and tolerances together. A cross-reference is a starting point for review, not an automatic substitution.
Explore Other Standards
ISO 6207:1992
ASTM B161
ASTM B163
ASTM B165
ASTM B167
ASTM B444
ASTM B622
ASTM B829
ASTM B704
BS EN 10216-5