ISO 6207:1992 is the International Standard for seamless nickel and nickel alloy tube, issued as a first edition on 15 July 1992. It covers round seamless tube for general purposes and for condenser and heat-exchanger applications, and it is the route into nickel alloys for drawings and purchase orders that cite ISO rather than ASTM or EN.
The standard identifies alloys by ISO NW numbers (NW2200, NW4400, NW6625 and so on), not by UNS numbers. Composition is taken from ISO 9722, tensile properties are set out in Table 2, and dimensional tolerances, U-bend limits and marking rules follow in the later clauses. That structure makes ISO 6207 a complete ordering specification rather than a single-property table.
This guide walks through the scope and size limits, the NW designation system, the composition basis, the tensile and hardness requirements, the tolerance tables and the information a purchase order has to state. Every value below is quoted from the standard itself.
ISO 6207:1992 at a Glance
| Standard | ISO 6207:1992(E), first edition, 15 July 1992 |
| Title | Seamless nickel and nickel alloy tube |
| Product | Round seamless tube, general purposes plus condenser and heat-exchanger service; U-bend tube included |
| Alloy identification | ISO NW numbers and descriptions, assigned under ISO/TR 7003 and ISO/TR 9721 |
| Composition source | Table 1, taken from ISO 9722 |
| Mechanical properties | Table 2, tensile properties and allowable fibre stress for hydrostatic testing |
| Tolerances | Tables 3 and 4 (diameter and wall), Table 5 (exact length) |
| U-bend rules | Tables 6 to 10 (bend radius, hardness, leg spacing, leg length, squareness) |
Scope and Size Range
Clause 1.1 applies the standard to round seamless nickel and nickel alloy tube in two service groups: tube for general purposes, and tube for condensers and heat exchangers. Clause 1.2 adds dimensional requirements and limiting bend radii for U-bend heat-exchanger tube of outside diameter up to and including 26 mm.
| Product group | Delivery condition | Outside diameter | Wall thickness |
|---|---|---|---|
| Tube for general purposes | Cold worked | 4 mm to 240 mm | As ordered (nominal or minimum) |
| Tube for general purposes | Hot worked | 38 mm to 240 mm | As ordered (nominal or minimum) |
| Condenser and heat-exchanger tube | Cold worked | Maximum 80 mm | Up to and including 5 mm |
| U-bend heat-exchanger tube | Cold worked | Up to and including 26 mm | Subject to Table 6 bend limits |
ISO 6207 also fixes the vocabulary used throughout the specification. A heat is the product of a furnace melt, or of several melts mixed before casting. A thick-wall tube has a specified wall above 3 % of the specified outside diameter; a thin-wall tube is at or below 3 %. A lot is tube of the same cross-sectional dimensions from the same heat, heat treated together or sequentially in a continuous furnace within 16 hours of production; where tubes cannot be identified by heat, a lot may not exceed 250 kg of material in the same heat-treated condition and size.
Alloy Designation: What the NW Number Means
ISO 6207 does not use UNS numbers. Alloys are identified by an NW number plus an ISO description, following the designation principles of ISO/TR 7003 and the chemical-symbol code of ISO/TR 9721. The four digits after NW are an ISO registry number — they are not a UNS number with a prefix, and two alloys with similar digits are not interchangeable. A conversion to ASTM or EN grades has to be made through the official cross-reference route and confirmed on the mill certificate.
| NW number | ISO description | Density (g/cm³, reference) |
|---|---|---|
| NW2200 | Ni99.0 | 8.9 |
| NW2201 | Ni99.0-LC | 8.9 |
| NW4400 | NiCu30 | 8.8 |
| NW4402 | NiCu30-LC | 8.8 |
| NW6600 | NiCr15Fe8 | 8.4 |
| NW6602 | NiCr15Fe8-LC | 8.4 |
| NW6601 | NiCr23Fe15Al | 8.0 |
| NW6625 | NiCr22Mo9Nb | 8.5 |
| NW6621 | NiCr20Ti | 8.4 |
| NW6455 | NiMo16Cr16Ti | 8.6 |
| NW8022 | NiCr21Mo14W | 8.7 |
| NW8002 | NiCr21Fe18Mo | 8.2 |
| NW6007 | NiCr22Fe20Mo6Cu2Nb | 8.3 |
| NW8985 | NiCr22Fe20Mo7Cu2 | 8.3 |
| NW6633 | NiCr28Fe20Co3Mo3W3 | 8.0 |
| NW6690 | NiCr29Fe | 8.2 |
| NW8825 | NiFe30Cr21Mo3 | 8.1 |
| NW8617 | NiCr22Co12Mo9 | 8.4 |
| NW7263 | NiCo20Cr20MoTi2Al | 8.4 |
| NW0276 | NiMo16Cr15FeW4 | 8.9 |
| NW0665 | NiMo28 | 9.2 |
| NW0001 | NiMo30Fe5 | 9.2 |
| NW8028 | FeNi31Cr27Mo4Cu1 | 8.0 |
| NW8800 | FeNi32Cr21AlTi | 8.0 |
| NW9810 | FeNi32Cr21AlTi-HC | 8.0 |
| NW9811 | FeNi32Cr21AlTi-HT | 8.0 |
| NW8801 | FeNi32Cr20Ti | 8.0 |
| NW9920 | FeNi35Cr20Cu4Mo2 | 8.1 |
Table 1 lists 28 alloys. Density values are averages given for information only and are not acceptance criteria.
Chemical Composition
Composition limits come from ISO 9722 and are reproduced in Table 1. Single values are maximum limits, except for nickel where a single value is a minimum; paired values are ranges. Nickel shown as “Remainder” is calculated by difference from 100 %. The limits do not preclude the presence of other unspecified elements, but any additional limit the purchaser needs has to be agreed with the supplier. Where no cobalt limit is given, cobalt up to 1.5 % is allowed and counted as nickel, in which case the cobalt content need not be reported.
| NW | C | Cr | Ni | Mo | Cu | Fe | Mn | Si | S | Other |
|---|---|---|---|---|---|---|---|---|---|---|
| NW2200 | 0.15 | — | 99.0 min | — | 0.2 | 0.4 | 0.3 | 0.3 | 0.010 | — |
| NW4400 | 0.30 | — | 63.0 min | — | 28.0–34.0 | 2.5 | 2.0 | 0.5 | 0.025 | — |
| NW6600 | 0.15 | 14.0–17.0 | 72.0 min | — | — | 6.0–10.0 | 1.0 | 0.5 | 0.015 | — |
| NW6625 | 0.10 | 20.0–23.0 | Remainder | 8.0–10.0 | — | 5.0 | 0.5 | 0.5 | 0.015 | P 0.015; Ti 0.40; Nb+Ta 3.15–4.15 |
| NW8022 | 0.015 | 20.0–22.5 | Remainder | 12.5–14.5 | — | 2.0–6.0 | 0.5 | 0.08 | 0.02 | P 0.02; W 2.5–3.5; V 0.35 |
| NW6455 | 0.015 | 14.0–17.0 | Remainder | 14.0–17.0 | — | 3.0 | 1.0 | 0.08 | 0.03 | Ti 0.7 |
Selected grades from Table 1 (compositions in % m/m). The full table, including Ni-Cr-Fe, Ni-Fe-Cr and Ni-Mo families, occupies pages 9–10 of the PDF.
Mechanical Properties
Table 2 sets minimum tensile strength (Rm), 0.2 % proof stress (Rp0.2) and elongation (A4) for each alloy and temper, and adds the allowable fibre stress Rf used to calculate hydrostatic test pressure. Elongation is measured on a gauge length of 4D, and proof stress follows the 0.2 % offset method of ISO 6892; a 1 % proof stress (Rp1.0) is reported only when the purchase order asks for it.
| NW | Temper | Size | Rm min (N/mm²) | Rp0.2 min (N/mm²) | A4 min (%) |
|---|---|---|---|---|---|
| NW2200 | Cold worked, annealed | D ≤ 125 mm | 380 | 105 | 35 |
| NW2200 | Cold worked, stress relieved | All sizes | 450 | 275 | 15 |
| NW2201 | Cold worked, annealed | D ≤ 125 mm | 350 | 85 | 35 |
| NW4400 | Cold worked, annealed | D ≤ 125 mm | 480 | 190 | 35 |
| NW4400 | Cold worked, stress relieved | All sizes | 590 | 380 | 15 |
| NW6600 | Cold worked, annealed | D ≤ 125 mm | 550 | 240 | 30 |
| NW6625 | Cold worked, annealed | All sizes | 830 | 415 | 30 |
| NW6625 | Cold worked, solution treated | All sizes | 690 | 275 | 30 |
| NW8022 | Hot worked, annealed | All sizes | 690 | 310 | 45 |
| NW6455 | Cold worked, solution treated | All sizes | 690 | 275 | 40 |
| NW6621 | Cold worked, annealed | δ ≤ 0.5 mm | 880–930 | 300 | 30 |
D is outside diameter and δ is wall thickness. Where two size bands are listed in Table 2 (for example D ≤ 125 mm and D > 125 mm), the lower strength band applies above 125 mm — check the table before releasing a purchase order for large-diameter tube.
Dimensional Tolerances
Tolerances depend on the forming route. Cold-worked tube follows Table 3, hot-worked tube follows Table 4, and both are subject to the ovality and concentricity clauses of 6.1.7. Wall thickness may be ordered as a nominal wall with plus/minus tolerance, or as a minimum wall with plus tolerance only; the two routes use different columns and must not be mixed on one order.
| Form | Outside diameter (mm) | OD tolerance (mm, ±) | Wall tolerance | Minimum wall tolerance |
|---|---|---|---|---|
| Cold worked | 4 to 16 | 0.15 | ±12.0 % | +25 % / −0 |
| Cold worked | 16 to 38 | 0.20 | ±10 % | +22 % / −0 |
| Cold worked | 38 to 90 | 0.25 | ±10 % | +22 % / −0 |
| Cold worked | 90 to 115 | 0.40 | ±10 % | +22 % / −0 |
| Cold worked | 115 to 150 | 0.50 | ±12.5 % | +25 % / −0 |
| Cold worked | 150 to 170 | 0.60 | ±12.5 % | +25 % / −0 |
| Cold worked | 170 to 210 | 0.70 | ±12.5 % | +25 % / −0 |
| Cold worked | 210 to 240 | 0.90 | ±12.5 % | +25 % / −0 |
| Hot worked | 38 to 50 | 0.6 | ±12.5 % | — |
| Hot worked | 50 to 60 | 0.7 | ±12.5 % | — |
| Hot worked | 60 to 140 | 0.8 | ±12.5 % | — |
| Hot worked | 140 to 240 | 1.2 | ±12.5 % | — |
Exact length follows Table 5: up to 9 000 mm the tolerance is +4/0 mm, from 9 000 to 12 000 mm it is +7/0 mm, from 12 000 to 15 000 mm it is +10/0 mm, and above 15 000 mm it is +13/0 mm. Tube ordered to a specified length is measured against these limits, not against a mill length range.
Condenser, Heat-Exchanger and U-Bend Tube
Clause 6.2 adds requirements that apply only to condenser and heat-exchanger tube, and clause 6.2.1 lists the alloys for which they apply: NW2200, NW2201, NW6600, NW6690, NW6625, NW4400, NW8825, NW8800, NW9810 and NW9811, each in its appropriate heat-treatment condition.
Two tests matter in practice. Every tube must pass a drift expanding test — expanded without rupture until the outside diameter has increased by 30 % (6.2.4). Stress-relieved tube supplied with annealed ends must also meet a hardness ceiling on those ends: the annealed end may not exceed the values in Table 7, measured by either Vickers or Rockwell at the supplier’s option.
| Alloy | Vickers hardness, max | Rockwell hardness, max |
|---|---|---|
| NW2200 (Ni99.0) | 116 HV | 65 HRB |
| NW2201 (Ni99.0-LC) | 112 HV | 62 HRB |
| NW4400 (NiCu30) | 137 HV | 75 HRB |
For U-bend tube, Table 6 fixes the minimum bend radius from the tube size and mean wall, with separate columns for annealed and stress-relieved tube. Table 8 then limits leg spacing to ±1.5 mm for a centreline bend radius up to 500 mm, ±2.5 mm from 500 to 750 mm and ±3.5 mm from 750 to 1 000 mm. Leg length follows Table 9 (+4/0 up to 7 m, +5/0 to 10 m, +7/0 to 19 m, +10/0 above 19 m) and the difference in length between the two legs of one tube may not exceed 4 mm. Squareness of ends is 0.3 mm up to 16 mm outside diameter and 0.5 mm above that.
Hydrostatic Test and Allowable Fibre Stress
Tube of 4 mm outside diameter and above, with wall of 0.4 mm and above, is hydrostatically tested at 70 bar gauge, provided the fibre stress calculated from the formula does not exceed the allowable fibre stress Rf in Table 2. The holding time is at least 20 seconds. Test pressure in bar is calculated as p = 20 Rf δmin / D, where δmin is the minimum wall after applying the minus tolerance and D is the specified outside diameter. By agreement the test pressure may rise to 1.5 times the allowable fibre stress; stress-relieved tube with annealed ends is tested before the ends are annealed.
Where a pneumatic test, eddy-current test or other non-destructive examination is required instead of the hydrostatic test, the method and acceptance standard must be agreed between purchaser and supplier and written into the order. Retests follow clause 9.11: two further samples from the same lot are tested, and the lot is accepted only if both pass.
What to Put on the Purchase Order
Clause 5 lists the information an ISO 6207 order has to carry. Missing items are a common cause of mill queries and rework, so the checklist is worth keeping with the RFQ:
- The number of the International Standard: ISO 6207:1992.
- Whether the tube is for general purposes or for condensers and heat exchangers.
- Quantity, expressed as mass, number of pieces or total length.
- Alloy identification — NW number or ISO description.
- Alloy temper, selected from Table 2.
- Dimensions: outside diameter with nominal wall thickness, or outside diameter with minimum wall thickness.
- Optional requirements where needed: ends other than plain-cut and deburred, straightness, annealed ends on stress-relieved tube, samples for product analysis, 1 % proof stress, a pressure test other than the standard one, non-destructive testing, individual tube marking, purchaser or third-party inspection, and a declaration of conformity.
- For U-bend tube: the bend limits, whether the U-bend area is to be stress relieved, the bend radius and leg length, whether wall-thickness proof in the bend is required, and whether hydrostatic testing is applied after bending.
Marking, Inspection and Conformity
Each bundle or shipping container is marked with the standard number, alloy identification, heat-treatment condition, size, gross and net mass, consignor and consignee, contract or order number, and any other information required by the contract. Individual tube marking with the standard number and alloy identification is applied when agreed. One-site inspection by the purchaser or a third party is carried out under the agreement in the contract, and the declaration of conformity required by clause 12 has to include the results of all tests called for by the standard and by the order.
Frequently Asked Questions
Is ISO 6207 the same as ASTM B161, B163 or B165?
No. They cover similar products through different systems. ISO 6207 identifies alloys by NW numbers and takes composition from ISO 9722; the ASTM specifications use UNS numbers and their own composition and test tables. Tensile requirements are close but not identical, and the tolerance and marking clauses differ. Order against the standard named on the drawing, and treat any conversion as an engineering decision recorded on the order, not as an automatic substitution.
Can an NW number be converted to a UNS number by reading the digits?
No. NW designations follow ISO/TR 7003 and the chemical-symbol code of ISO/TR 9721; the digits are an ISO registry number, not a UNS number. For example NW6625 (NiCr22Mo9Nb) corresponds in chemistry to the alloy commonly sold as UNS N06625, but that equivalence has to be confirmed through the official cross-reference and the mill certificate rather than assumed from the number.
Which temper should be specified for heat-exchanger tube?
Most condenser and heat-exchanger orders call for cold-worked, annealed tube, or for cold-worked stress-relieved tube with annealed ends. The second option carries the Table 7 hardness ceiling on the annealed ends (116 HV for NW2200, 112 HV for NW2201, 137 HV for NW4400). If the tube will be U-bent, state whether the bend area is to be stress relieved and whether the wall thickness in the bend has to be proved.
What wall thickness tolerance applies to cold-worked tube?
Table 3 gives plus/minus 12 % on nominal wall for outside diameter 4 to 16 mm, plus/minus 10 % from 16 to 115 mm, and plus/minus 12.5 % above 115 mm. If a minimum wall is ordered instead, the tolerance is +22 %/−0 up to 115 mm and +25 %/−0 above. Choose one route on the order; mixing nominal and minimum wall columns is not permitted.
Does ISO 6207 require a hydrostatic test on every tube?
Yes for tube of 4 mm outside diameter and above with wall of 0.4 mm and above, unless a pneumatic or eddy-current test has been agreed as an alternative. The standard test pressure is 70 bar gauge, capped by the allowable fibre stress in Table 2, and the hold time is at least 20 seconds.
Explore Other Standards
ASTM B161
ASTM B163
ASTM B165
ASTM B167
ASTM B444
ASTM B622
ASTM B829
DIN 17751:2002-09
ISO 15156-3:2020
BS EN 10216-5